Impurity removal method for dichloromolybdenum dioxide product
Through three heat treatment methods, especially the reduction of vanadium tetrachloride in a hydrogen atmosphere, the problem of difficult removal of vanadium impurities in molybdenum dichloride products has been solved, and the product purity has been significantly improved, meeting the purity requirements of chip products and suitable for large-scale production Production.
Patent Information
- Application Number
- CN202411088878.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-18
AI Technical Summary
Existing technology is difficult to effectively remove vanadium impurities in molybdenum dichloride products, resulting in its purity failing to meet the requirements of chip products. In particular, the boiling point of vanadium tetrachloride is close to the sublimation temperature of molybdenum dichloride, making it difficult to pass through ordinary sublimation. Complete removal of impurities.
Three heat treatment methods are adopted, in which the first heat treatment removes low sublimation point impurities, the second heat treatment reduces vanadium tetrachloride in a hydrogen atmosphere to increase its sublimation temperature, and the third heat treatment sublimates molybdenum dichloride and separates it. Remove impurities, significantly reduce vanadium-containing impurities, and improve product purity.
Through this method, the vanadium impurity content in molybdenum dichloride products is significantly reduced, reaching a removal rate of more than 90%, the purity meets the requirements of chip products, the operation is simple, and it is suitable for large-scale production.
Smart Images

Figure CN118791044A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of molybdenum dioxide dichloride products, and particularly relates to a method for removing impurities from molybdenum dioxide dichloride products. Background Art
[0002] Molybdenum dioxide dichloride, with the chemical formula of MoO2Cl2, is a light yellow crystal with a sublimation temperature of 159°C. It is highly hygroscopic and easily hydrolyzed. It is currently generally used as a molybdenum source material for chemical vapor deposition (CVD) to deposit molybdenum films, which can be used as diffusion barriers, electrodes, interconnects and other devices. Molybdenum dioxide dichloride is widely used in memory chips, logic chips, catalysts and other chip semiconductor industries due to its high conformality and suitability for mass production.
[0003] At present, the methods for synthesizing molybdenum dioxide dichloride mainly include chlorination reaction method, sublimation purification method, oxyhalogen compound chemical method, etc. The application of molybdenum dioxide dichloride in high-end chips has higher and higher requirements for purity. However, due to the co-existence of vanadium and molybdenum minerals, molybdenum dioxide dichloride products synthesized by various synthesis methods have a high content of vanadium-containing impurities remaining. Using the ordinary sublimation impurity removal method, the purity of the molybdenum dioxide dichloride product after impurity removal still cannot reach the level required for application in chip products. For example, the vanadium tetrachloride impurity in the molybdenum dioxide dichloride product, the boiling point of vanadium tetrachloride is 148.5℃, and the sublimation temperature of vanadium tetrachloride and molybdenum dioxide dichloride is close, and it cannot be completely removed by ordinary sublimation impurity removal. Summary of the invention
[0004] In view of the difficulty in removing vanadium-containing impurities from molybdenum dioxide dichloride products involved in the above-mentioned prior art, the present invention provides a method for removing impurities from molybdenum dioxide dichloride products.
[0005] To achieve the above purpose, the following technical solutions are specifically included:
[0006] A method for removing impurities from a molybdenum dioxide dichloride product comprises the following steps:
[0007] (1) placing a molybdenum dioxide dichloride product at one end of a tubular container, introducing an inert gas into one end of the molybdenum dioxide dichloride product, and performing a first heat treatment to obtain a product after the first heat treatment;
[0008] (2) introducing hydrogen into one end of the product after the first heat treatment to perform a second heat treatment to obtain a product after the second heat treatment;
[0009] (3) introducing an inert gas into one end of the product after the second heat treatment, and performing a third heat treatment to obtain a molybdenum dioxide dichloride product after impurities are removed.
[0010] In the method of the present invention, firstly, impurities with low sublimation points are removed in the first heat treatment; secondly, hydrogen is introduced to perform the second heat treatment on the molybdenum dioxide dichloride product, the product is completely sublimated in the hydrogen atmosphere, the chloride containing vanadium impurity elements (such as vanadium tetrachloride) in the product is reduced, the valence state of the chloride containing vanadium impurity elements is reduced, and the sublimation temperature thereof is increased. At this time, the sublimation temperature of the chloride containing vanadium impurity elements is higher than that of molybdenum dioxide dichloride; finally, the third heat treatment is performed to sublime the molybdenum dioxide dichloride, and impurities with higher sublimation temperature than that of molybdenum dioxide dichloride remain in the original place without sublimation, so that the impurities in the molybdenum dioxide dichloride product can be effectively separated and removed, especially the vanadium impurities in the product are significantly reduced, the purity of the molybdenum dioxide dichloride product is significantly improved, and the molybdenum dioxide dichloride product after impurity removal meets the purity requirements for application in chip products; the method of the present invention is simple to operate, high in efficiency, and easy to be mass-produced.
[0011] Preferably, in step (1), the temperature of the first heat treatment is 120-130° C., and the time of the first heat treatment is 2-4 hours.
[0012] At the above-mentioned heat treatment temperature, impurities having a lower sublimation temperature than molybdenum dioxide dichloride can be effectively separated and removed.
[0013] Preferably, in step (1), the content of vanadium in the molybdenum dichloride product is ≥300 ppb, the material of the tubular container is quartz, the diameter of the tubular container is 100-200 mm, and the length of the tubular container is 1.8-2.2 m.
[0014] The method of the present invention is more suitable for removing impurities from a molybdenum dioxide dichloride product with a high vanadium (such as vanadium tetrachloride) impurity content. The impurity removal method of the present invention can reduce the molybdenum dioxide dichloride product with a vanadium content of ≥300 ppb to a vanadium content of ≤20 ppb, and the removal rate of vanadium impurities reaches more than 90%.
[0015] Preferably, in step (1), the flow rate of the inert gas is 150-300 L / h.
[0016] By introducing and discharging an appropriate flow of inert gas, the sublimated impurities can be discharged in time, effectively promoting the separation and removal of low sublimation point impurities in the product.
[0017] Preferably, in step (1), the inert gas includes at least one of nitrogen, argon and helium.
[0018] Preferably, in step (2), the temperature of the second heat treatment is 250-400° C., and the time of the second heat treatment is 2-4 hours.
[0019] At the above-mentioned second heat treatment temperature, vanadium-containing chloride impurities such as vanadium tetrachloride in the molybdenum dioxide dichloride product can be effectively reduced, so that the sublimation temperature (>400°C) of the reduced vanadium-containing chloride impurities is much higher than that of molybdenum dioxide dichloride, which facilitates the subsequent sublimation separation of the reduced vanadium-containing chloride impurities and molybdenum dioxide dichloride.
[0020] Preferably, in step (2), the flow rate of hydrogen is 100-200 L / h.
[0021] Under the above-mentioned hydrogen flow rate, the reduction efficiency and the flow rate of hydrogen in a container of a certain volume are regulated by the hydrogen flow rate, thereby achieving the control of the sublimation and condensation rates of the molybdenum dioxide dichloride product. When the sublimation rate of the molybdenum dioxide dichloride product is between 0.5 and 3 kg / h, the hydrogen reduction effect is more sufficient.
[0022] Preferably, the method further comprises repeating step (2), wherein the number of repetitions is ≥ 1 times.
[0023] The process of heat treatment in step (2) for the second time under a hydrogen atmosphere can be repeated to make the hydrogen reduction more thorough and further remove impurities.
[0024] Preferably, in step (3), the temperature of the third heat treatment is 160-250° C., and the time of the third heat treatment is 2-4 hours.
[0025] The temperature of the third heat treatment is not only higher than the sublimation temperature of molybdenum dioxide dichloride, but also much lower than the sublimation temperature of the reduced vanadium-containing chloride impurities, so that the reduced vanadium-containing chloride impurities can be effectively separated from molybdenum dioxide dichloride, and the molybdenum dioxide dichloride separated by sublimation is re-condensed and collected, thereby achieving the purpose of improving the purity of molybdenum dioxide dichloride.
[0026] Preferably, in step (3), the flow rate of the inert gas is 50-150 L / h.
[0027] Preferably, in step (3), the content of vanadium in the molybdenum dioxide dichloride product after impurity removal is ≤20ppb
[0028] Compared with the prior art, the present invention has the following beneficial effects: the present invention is heat treated three times, and the second heat treatment is carried out under a hydrogen atmosphere, which can effectively separate and remove impurities in the molybdenum dioxide dichloride product as a whole, especially significantly reduce the vanadium-containing impurities in the product, and significantly improve the purity of the molybdenum dioxide dichloride product, so that the molybdenum dioxide dichloride product after impurity removal meets the purity requirements for chip products; the method of the present invention is simple to operate, high in efficiency, and easy to scale up production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a schematic diagram of the first heat treatment for impurity removal according to the present invention.
[0030] Figure 2 It is a schematic diagram of the second heat treatment for impurity removal of the present invention. DETAILED DESCRIPTION
[0031] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below through specific examples. The test methods used in the examples and / or comparative examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified. Among them, the molybdenum dioxide dichloride raw material block is a commercially available product prepared by the chlorination method, and ICP-MS is used to detect and determine the V content of each substance.
[0032] Example 1
[0033] (1) Select a quartz tube with a diameter of 130 mm and a length of 2 m, clean it with aqua regia and ultrapure water, connect the gas pipeline to the quartz tube, weigh 5 kg of molybdenum dioxide dichloride raw material block (the V content is 2100 ppb as determined by the test) and put it into one end of the quartz tube, and seal the other end of the quartz tube;
[0034] (2) First, introduce nitrogen gas at a flow rate of 200 L / h into the quartz tube for 30 minutes to replace the air in the quartz tube, and continue to introduce nitrogen gas to exhaust the tail gas at the end away from the product. At the same time, the molybdenum dioxide dichloride block in the quartz tube is heat treated once. The schematic diagram is shown in the attached figure. Figure 1 As shown, the heat treatment condition is 120°C for 3 hours to remove low boiling point impurities (such as metal impurities such as titanium), and the process ends after natural cooling. According to ICP-MS detection, the V content in the molybdenum dioxide dichloride product after the first heat treatment is 1905 ppb.
[0035] (3) The molybdenum dioxide dichloride product after the first heat treatment is reloaded into a clean quartz furnace tube, and the air in the tube is replaced by nitrogen inert gas. The product end is heated for the second heat treatment, and hydrogen is introduced into one end of the product. The tail gas is discharged at the end away from the product. The hydrogen flow rate is maintained at 150L / h. The schematic diagram is shown in the attached figure. Figure 2 As shown, the second heat treatment temperature is 295°C, the time is 2-4h, and it is considered to be completed when the product is completely sublimated;
[0036] The heat causes molybdenum dioxide dichloride to vaporize and sublime. Driven by the hydrogen gas flow and the change in temperature, the molybdenum dioxide dichloride vapor is re-condensed at the other end of the quartz tube, and the vanadium tetrachloride mixed in the solid molybdenum dioxide dichloride is vaporized together with the hydrogen to generate low-valent vanadium;
[0037] (4) After the molybdenum dioxide dichloride product is reduced by hydrogen in step (3), nitrogen is introduced and the flow rate is maintained at 100 L / h, and the product end is heated for a third heat treatment at a temperature of 180° C. for 3 h;
[0038] The heat causes the molybdenum dioxide dichloride to vaporize and sublime, and driven by the nitrogen gas flow and the temperature change, after sublimation, the molybdenum dioxide dichloride vapor is re-condensed at the other end of the quartz tube. Since the vanadium impurity has a high sublimation temperature after reduction, it remains near the raw material, thereby achieving separation. The re-condensed molybdenum dioxide dichloride product is collected, that is, the molybdenum dioxide dichloride product after the third heat treatment. The V content is 15ppb after testing.
[0039] Example 2
[0040] (1) Select a quartz tube with a diameter of 130 mm and a length of 2 m, clean it with aqua regia and ultrapure water, connect the gas pipeline to the quartz tube, weigh 5 kg of molybdenum dioxide dichloride raw material block (the V content is 2080 ppb according to the test) and put it into one end of the quartz tube, and seal the other end of the quartz tube;
[0041] (2) First, introduce nitrogen gas at a flow rate of 200 L / h into the quartz tube for 30 minutes to replace the air in the quartz tube, and continue to introduce nitrogen gas to exhaust the tail gas at the end away from the product. At the same time, heat the molybdenum dioxide dichloride block in the quartz tube for a heat treatment. The schematic diagram is shown in the attached figure. Figure 1 As shown, the heat treatment condition is 130°C for 3 hours to remove low-boiling impurities, and the heat treatment ends after natural cooling. After testing, the V content in the molybdenum dioxide dichloride product after the first heat treatment is 1880ppb.
[0042] (3) The molybdenum dioxide dichloride product after the first heat treatment is reloaded into a clean quartz furnace tube, and the air in the tube is replaced by nitrogen inert gas. The product end is heated for the second heat treatment, and hydrogen is introduced into one end of the product. The hydrogen flow rate is maintained at 100L / h, and the tail gas is discharged at the end away from the product. The schematic diagram is shown in the attached figure. Figure 2 As shown, the second heat treatment temperature is 320°C, the time is 2-4h, and it is considered to be completed when the product is completely sublimated;
[0043] The heat causes molybdenum dioxide dichloride to vaporize and sublime. Driven by the hydrogen gas flow and the change in temperature, the molybdenum dioxide dichloride vapor is re-condensed at the other end of the quartz tube, and the vanadium tetrachloride mixed in the solid molybdenum dioxide dichloride is vaporized together with the hydrogen to generate low-valent vanadium;
[0044] (4) After the molybdenum dioxide dichloride product is reduced by hydrogen in step (3), nitrogen is introduced and the flow rate is maintained at 100 L / h, and the product end is heated for a third heat treatment, and the third heat treatment temperature is 190° C. and the time is 3 h;
[0045] The heat causes the molybdenum dioxide dichloride to vaporize and sublime, and driven by the nitrogen gas flow and the temperature change, after sublimation, the molybdenum dioxide dichloride vapor is re-condensed at the other end of the quartz tube. Since the vanadium impurity has a high sublimation temperature after reduction, it remains near the raw material, thereby achieving separation. The re-condensed molybdenum dioxide dichloride product is collected, that is, the molybdenum dioxide dichloride product after the third heat treatment. The V content is 10ppb as detected by ICP-MS.
[0046] Example 3
[0047] Compared with Example 1, this embodiment adds one more heat treatment under hydrogen atmosphere, and the rest is the same, as follows:
[0048] (1)-(3): Same as in Example 1;
[0049] (4) After replacing the air in the tube with nitrogen inert gas, start heating at the product end for the third heat treatment, and introduce hydrogen at one end of the product, exhaust the tail gas at the end away from the product, and maintain the hydrogen flow rate at 150L / h. The third heat treatment temperature is 295°C, the time is 2-4h, and the process is considered complete when the product is completely sublimated;
[0050] (5) After the molybdenum dioxide dichloride product is reduced by hydrogen in step (4), nitrogen is introduced and the flow rate is maintained at 100 L / h, and the product end is heated for a fourth heat treatment, the fourth heat treatment temperature is 180° C., and the time is 3 h; the molybdenum dioxide dichloride product after the fourth heat treatment is obtained, and the V content is 10 ppb as detected by ICP-MS.
[0051] Example 4
[0052] Compared with Example 1, the second heat treatment temperature in step (3) of this example is 250° C., and the rest is the same.
[0053] Example 5
[0054] Compared with Example 1, the second heat treatment temperature in step (3) of this example is 400° C., and the rest is the same.
[0055] Example 6
[0056] Compared with Example 1, the third heat treatment temperature in step (4) of this example is 162° C., and the rest is the same.
[0057] Example 7
[0058] Compared with Example 1, the third heat treatment temperature in step (4) of this example is 250° C., and the rest is the same.
[0059] Comparative Example 1
[0060] Compared with Example 1, in this comparative example, in step (3), the hydrogen gas is replaced by the inert gas nitrogen gas, and the rest is the same. The V content of the final product is detected by ICP-MS, as shown in Table 1.
[0061] Comparative Example 2
[0062] Compared with Comparative Example 1, this comparative example takes the product in Comparative Example 1 and performs a normal sublimation treatment again. The specific steps are as follows:
[0063] (1) Place the final product of Comparative Example 1 into one end of a clean quartz tube (same style as Example 1), and seal the other end of the quartz tube;
[0064] (2) Nitrogen gas at a flow rate of 200 L / h was introduced into the quartz tube for 30 min to replace the air in the quartz tube, and nitrogen gas was continuously introduced to exhaust the tail gas at the end away from the product. At the same time, the molybdenum dioxide dichloride block in the quartz tube was subjected to a heat treatment at 120° C. for 3 h, and then naturally cooled to terminate. The V content of the final product was detected by ICP-MS, as shown in Table 1.
[0065] Table 1
[0066]
[0067] Among them, the vanadium removal rate of the first heat treatment (%) = c1 (V content in the raw material) - c2 (V content in the molybdenum dioxide dichloride product after the first heat treatment) / c1 (V content in the raw material) * 100%; the final vanadium removal rate (%) = c1 (V content in the raw material) - c3 (V content in the final molybdenum dioxide dichloride product) / c1 (V content in the raw material) * 100%.
[0068] It can be seen from the above embodiments that the impurity removal method of the present invention can reduce the vanadium impurity content in the molybdenum dioxide dichloride product to below 20 ppb, thereby obtaining a high-purity molybdenum dioxide dichloride product that meets the purity requirements for application in chip-level products.
[0069] As can be seen from Examples 1 and 2, the purpose of the first heat treatment is to remove impurities with low sublimation temperatures, and the temperature is generally 120-130°C, which can ensure that the sublimation temperature of impurities with low sublimation temperatures is reached, and the sublimation temperature of vanadium tetrachloride and molybdenum dioxide dichloride is not reached, so as to effectively separate and remove impurities with low sublimation temperatures in the product. The temperature of the second heat treatment process is maintained at 250-400°C, which is suitable for ensuring the gasification efficiency of the product, and can also make the vanadium impurities fully react with hydrogen, so as to facilitate the condensation of gaseous products in the container. As can be seen from Examples 1 and 4-5, with the increase of the temperature of the second heat treatment, it is more conducive to hydrogen reduction and the vanadium removal rate increases. It can be seen from Examples 1 and 6-7 that as the temperature of the third heat treatment increases, the greater the difference between the temperature of the third heat treatment and the sublimation point of molybdenum dioxide dichloride, although both are sufficient to completely sublimate molybdenum dioxide dichloride, the higher the temperature, the closer it will be to the temperature at which impurities sublimate, increasing the probability of sublimation of some vanadium-containing impurities, resulting in a decrease in the vanadium removal rate. Therefore, in the method of the present invention, when the temperature of the third heat treatment is 160-250°C, the temperature is suitable, ensuring that it is higher than the sublimation temperature of molybdenum dioxide dichloride and lower than the sublimation temperature of vanadium impurities, so that vanadium impurities are effectively separated from molybdenum dioxide dichloride, and it is also convenient for the gaseous product to be condensed in the container, and the vanadium removal effect is better.
[0070] It can be seen from Example 1 and Comparative Examples 1-2 that without the second heat treatment of hydrogen reduction, even if the number of heat treatments or sublimations is increased, the vanadium impurity in the final molybdenum dioxide dichloride product cannot be reduced to below 100 ppb.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for removing impurities from a molybdenum dioxide dichloride product, characterized in that: The steps include: (1) placing a molybdenum dioxide dichloride product at one end of a tubular container, introducing an inert gas into one end of the molybdenum dioxide dichloride product, and performing a first heat treatment to obtain a product after the first heat treatment; (2) introducing hydrogen into one end of the product after the first heat treatment to perform a second heat treatment to obtain a product after the second heat treatment; (3) introducing an inert gas into one end of the product after the second heat treatment, and performing a third heat treatment to obtain a molybdenum dioxide dichloride product after impurities are removed.
2. The impurity removal method of molybdenum dioxide dichloride product as claimed in claim 1, characterized in that, In step (1), the temperature of the first heat treatment is 120-130° C., and the time of the first heat treatment is 2-4 hours.
3. The impurity removal method of molybdenum dioxide dichloride product as claimed in claim 1, characterized in that, In step (2), the temperature of the second heat treatment is 250-400° C., and the time of the second heat treatment is 2-4 hours.
4. The impurity removal method of molybdenum dioxide dichloride product as claimed in claim 1, characterized in that, In step (3), the temperature of the third heat treatment is 160-250° C., and the time of the third heat treatment is 2-4 hours.
5. The impurity removal method of the molybdenum dioxide dichloride product as claimed in claim 1, characterized in that, In step (1), the flow rate of the inert gas is 150-300 L / h.
6. The impurity removal method of the molybdenum dioxide dichloride product as claimed in claim 1, characterized in that: In step (2), the flow rate of hydrogen is 100-200 L / h.
7. The impurity removal method of the molybdenum dioxide dichloride product as claimed in claim 1, characterized in that: In step (3), the flow rate of the inert gas is 50-150 L / h.
8. The impurity removal method of the molybdenum dioxide dichloride product as claimed in claim 1, characterized in that: In step (1), the content of vanadium in the molybdenum dichloride product is ≥300 ppb, the material of the tubular container is quartz, the diameter of the tubular container is 100-200 mm, and the length of the tubular container is 1.8-2.2 m.
9. The impurity removal method of molybdenum dioxide dichloride product as claimed in claim 1, characterized in that, Step (2) also includes repeating the process of step (2), with the number of repetitions being ≥ 1 times.
10. The impurity removal method of the molybdenum dioxide dichloride product as claimed in claim 1, characterized in that: In step (3), the content of vanadium in the molybdenum dioxide dichloride product after impurities removal is ≤20ppb.
Citation Information
Cited By
Molybdenum dioxide dichloride preparation method based on molybdenum-containing solution
CN119774661A
A method for preparing molybdenum dioxide dichloride based on molybdenum-containing solution
CN119774661B