Impact-resistant gypsum board and preparation method thereof

By combining phosphorus-containing modified polypropylene fiber and DOPO-containing modified carbon oxide fiber with gypsum powder, it forms impact-resistant gypsum board, which solves the shortcomings of fiber gypsum board in terms of impact resistance and fire-infection stability, and achieves efficient material resistance Impact and good fire-to-fire performance.

CN118791279BActive Publication Date: 2024-11-26HUNAN CONSTR ENG HUIJIAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411288039.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-26
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

Existing fiber gypsum boards have shortcomings in impact resistance and fire-infection stability, and cannot meet the growing demand.

Method used

The phosphorus-containing modified polypropylene fiber and DOPO-containing modified carbon oxide fiber are combined with gypsum powder, and then pressed in a plastic molding machine after stirring evenly to form impact-resistant gypsum boards, which are used to improve the flame retardant mechanism of phosphorus, nitrogen and silicon elements. The material's fire-touch stability and enhances impact resistance through the three-dimensional network structure of the fiber.

Benefits of technology

The prepared impact gypsum board has excellent impact resistance and fire stability. It effectively insulates energy transmission through the formation of phosphoric acid, carbon layer and flame-retardant gas, which significantly improves the compressive strength and flexural strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

The invention relates to the technical field of gypsum boards, and discloses an impact-resistant gypsum board and a preparation method thereof. The invention uses 4-vinylphenol and hexachlorocyclotriphosphazene as raw materials, and obtains an intermediate through reaction. The alkenyl contained in the intermediate is used to carry out a grafting reaction with polypropylene fiber under the initiation of benzoyl peroxide to obtain phosphorus-containing modified polypropylene fiber. DOPO and trimethoxyvinylsilane are used as raw materials, and phosphorus-containing silane is obtained through reaction. The active functional groups on the surface of oxidized carbon fiber are used, and phosphorus-containing silane is used as a grafting monomer to perform surface modification to obtain DOPO-modified oxidized carbon fiber. Finally, phosphorus-containing modified polypropylene fiber, DOPO-modified oxidized carbon fiber, etc. are added to gypsum powder, stirred and mixed evenly, pressed, and formed to obtain an impact-resistant gypsum board. The gypsum board prepared by the invention has excellent impact resistance and fire stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gypsum boards, in particular to an impact-resistant gypsum board and a preparation method thereof. Background Art

[0002] Gypsum board has the characteristics of light weight, high strength and thin thickness. It is widely used in decorative panels such as interior partitions and ceilings of residential buildings, office buildings, etc. At present, paper-faced gypsum board and fiber gypsum board are more commonly used. The surface paper of paper-faced gypsum board is easy to fall off, which affects its service life, while the fiber gypsum board has a firm internal bond and has high bending strength and bonding strength, which is better than paper-faced gypsum board. However, with the continuous development of science and technology, ordinary fiber gypsum board can no longer meet people's needs. Based on this, the study of the impact resistance of fiber gypsum board is one of the hot spots of current researchers.

[0003] Polypropylene fiber is a synthetic fiber obtained by spinning polypropylene from propylene polymerization. It has excellent characteristics such as high strength, wear resistance, and corrosion resistance. It is widely used in chemical industry, environmental protection, new energy and other fields. Carbon fiber refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It is made of acrylic and viscose fibers and is oxidized and carbonized at high temperature. It is widely used in aerospace and other fields.

[0004] For example, the patent application publication number CN 117024100 A discloses a production formula and production method of a plasticized gypsum board. The invention uses gypsum powder, carbon fiber, etc. as raw materials, and the gypsum board prepared has good impact resistance, but its fire stability is poor. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides an impact-resistant gypsum board and a preparation method thereof. The gypsum board prepared by the present invention has excellent impact resistance and flame retardant effects.

[0006] The present invention is achieved through the following technical solutions:

[0007] An impact-resistant gypsum board, comprising the following components by weight: 100 parts of gypsum powder, 0.05-0.1 parts of gypsum retarder, 60-80 parts of deionized water, 1-20 parts of phosphorus-modified polypropylene fiber, and 1-20 parts of DOPO-modified oxidized carbon fiber;

[0008] Wherein, the preparation method of the impact-resistant gypsum board is:

[0009] Add gypsum powder and gypsum retarder to deionized water, stir and disperse, then add phosphorus-modified polypropylene fiber and DOPO-modified oxidized carbon fiber, stir and mix evenly, pour the mixture into a mold, and press in a plastic compression molding machine, wherein the pressure is 0.2-0.3MPa, the pressurization time is 20-30min, after the pressing is completed, place it at room temperature for 12-24h, dry, and mold to obtain an impact-resistant gypsum board;

[0010] The preparation method of the phosphorus-containing modified polypropylene fiber is:

[0011] (1) Add 4-vinylphenol to tetrahydrofuran solvent, stir and disperse, then add hexachlorocyclotriphosphazene, stir and mix evenly, heat to 60-75°C, reflux for 40-80h, wash and dry after the reaction, and obtain an intermediate, whose structural formula is , the mass ratio of 4-vinylphenol to hexachlorocyclotriphosphazene is 180-240:100;

[0012] (2) Under nitrogen conditions, adding polypropylene fiber to methanol solvent, stirring and dispersing, then adding intermediate and benzoyl peroxide thereto, stirring evenly, heating to 80-90° C., reacting for 6-12 hours, cooling to room temperature after the reaction, washing with acetone, and drying to obtain phosphorus-containing modified polypropylene fiber, wherein the mass ratio of the polypropylene fiber, intermediate, and benzoyl peroxide is 100:100-200:2-5;

[0013] The preparation method of the DOPO-modified oxidized carbon fiber is as follows:

[0014] S1. Under nitrogen conditions, DOPO and trimethoxyvinylsilane are added to a chloroform solvent, stirred and dispersed, and then azobisisobutyronitrile is added thereto, and the reaction is carried out at 75-85° C. for 12-24 hours. After the reaction is completed, the phosphorus-containing silane is obtained by vacuum distillation, wherein the mass ratio of DOPO, trimethoxyvinylsilane and azobisisobutyronitrile is 100:50-80:0.7-1;

[0015] S2. Add oxidized carbon fiber to ethanol solvent, disperse by ultrasonic, add 10% hydrochloric acid to adjust the pH to 3-4, add phosphorus-containing silane to it, react at 60-80°C for 20-48h, wash with deionized water after the reaction, and dry to obtain DOPO-modified oxidized carbon fiber, wherein the mass ratio of oxidized carbon fiber to phosphorus-containing silane is 100:80-150.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0017] The present invention uses 4-vinylphenol and hexachlorocyclotriphosphazene as raw materials, and obtains an intermediate through reaction. The olefin group contained in the intermediate is used to carry out grafting reaction with polypropylene fiber under the initiation of benzoyl peroxide to obtain phosphorus-containing modified polypropylene fiber. DOPO and trimethoxyvinylsilane are used as raw materials, and phosphorus-containing silane is obtained through reaction. The hydroxyl group contained on the surface of oxidized carbon fiber is used, and phosphorus-containing silane is used as a grafting monomer to perform surface modification on the oxidized carbon fiber to obtain DOPO-containing modified oxidized carbon fiber. Finally, phosphorus-containing modified polypropylene fiber, DOPO-containing modified oxidized carbon fiber, etc. are added to gypsum powder, stirred and mixed evenly, pressed, and formed to obtain an impact-resistant gypsum board.

[0018] The impact-resistant gypsum board prepared by the present invention contains phosphorus, nitrogen and silicon, which are flame-retardant elements. The specific flame-retardant mechanism is as follows: phosphorus generates phosphoric acid, metaphosphoric acid and other substances when heated, which can promote the dehydration of the material into carbon, forming a dense carbon layer to isolate material transportation and energy transfer; when silicon is heated, it can form a dense carbon layer on the surface of the material, further isolating material transportation and energy transfer; when nitrogen is heated, it generates non-flammable gas to dilute the flammable gas in the air. The three elements assist each other and jointly improve the material's fire stability.

[0019] The impact-resistant gypsum board prepared by the present invention contains polypropylene fiber and carbon fiber. The two fibers are added to the gypsum powder, and can be mixed with each other to form a larger three-dimensional network structure. The fiber has high fracture toughness. When the gypsum matrix is ​​subjected to external force, the mixed fibers can absorb part of the energy to effectively reduce and inhibit the generation of matrix cracks, enhance the toughness of the gypsum, and improve the impact resistance. The gypsum board prepared by the present invention has excellent impact resistance and fire stability. DETAILED DESCRIPTION

[0020] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0021] Preparation route of oxidized carbon fiber: Place short-cut polyacrylonitrile-based carbon fiber in acetone solvent and soak for 24 hours. After soaking, wash with deionized water and dry. Then place it in 100mL of a mixed solution of concentrated sulfuric acid and concentrated nitric acid with a volume ratio of 3:1, stir and react at 80°C for 6 hours. After the reaction is completed, cool to room temperature, wash with deionized water, and dry to obtain oxidized carbon fiber.

[0022] The gypsum retarder is sodium citrate.

[0023] Example 1

[0024] (1) Add 5.4 g of 4-vinylphenol to tetrahydrofuran solvent, stir and disperse, then add 3 g of hexachlorocyclotriphosphazene, stir and mix evenly, heat to 65°C, reflux for 48 hours, and after the reaction is completed, wash and dry to obtain an intermediate.

[0025] (2) Under nitrogen conditions, 20 g of polypropylene fiber was added to methanol solvent and stirred to disperse. Then, 30 g of the intermediate and 0.5 g of benzoyl peroxide were added thereto and stirred evenly. The temperature was raised to 85 °C and the reaction was carried out for 12 h. After the reaction was completed, the mixture was cooled to room temperature, washed with acetone, and dried to obtain phosphorus-containing modified polypropylene fiber.

[0026] (3) Under nitrogen conditions, 10 g of DOPO and 6 g of trimethoxyvinylsilane were added to a chloroform solvent and stirred for dispersion. Then, 0.08 g of azobisisobutyronitrile was added thereto and the mixture was reacted at 80°C for 12 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain phosphorus-containing silane.

[0027] (4) Add 20 g of oxidized carbon fiber to ethanol solvent and disperse it ultrasonically. Then add 10% hydrochloric acid to adjust the pH to 4. Then add 20 g of phosphorus-containing silane and react at 70°C for 24 hours. After the reaction is completed, wash with deionized water and dry to obtain DOPO-modified oxidized carbon fiber.

[0028] (5) Add 100 g of gypsum powder and 0.06 g of gypsum retarder to 80 g of deionized water, stir and disperse, then add 1 g of phosphorus-containing modified polypropylene fiber and 1 g of DOPO-modified oxidized carbon fiber, stir and mix evenly, pour the mixture into a mold, and press it in a plastic compression molding machine at a pressure of 0.25 MPa for 25 min. After pressing, place it at room temperature for 20 h, dry it, and mold it to obtain an impact-resistant gypsum board.

[0029] Example 2

[0030] (1) Add 7.2 g of 4-vinylphenol to tetrahydrofuran solvent, stir and disperse, then add 3 g of hexachlorocyclotriphosphazene, stir and mix evenly, heat to 75°C, reflux for 40 hours, and after the reaction is completed, wash and dry to obtain an intermediate.

[0031] (2) Under nitrogen conditions, 20 g of polypropylene fiber was added to methanol solvent and stirred to disperse. Then, 25 g of the intermediate and 0.8 g of benzoyl peroxide were added thereto and stirred evenly. The temperature was raised to 85 °C and the reaction was carried out for 10 h. After the reaction was completed, the mixture was cooled to room temperature, washed with acetone, and dried to obtain phosphorus-containing modified polypropylene fiber.

[0032] (3) Under nitrogen conditions, 10 g of DOPO and 6 g of trimethoxyvinylsilane were added to a chloroform solvent and stirred for dispersion. Then, 0.08 g of azobisisobutyronitrile was added thereto and the mixture was reacted at 80°C for 24 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain phosphorus-containing silane.

[0033] (4) Add 20 g of oxidized carbon fiber to ethanol solvent and disperse it ultrasonically. Then add 10% hydrochloric acid to adjust the pH to 4. Then add 20 g of phosphorus-containing silane and react at 65°C for 48 hours. After the reaction is completed, wash with deionized water and dry to obtain DOPO-modified oxidized carbon fiber.

[0034] (5) Add 100 g of gypsum powder and 0.07 g of gypsum retarder to 65 g of deionized water, stir and disperse, then add 5 g of phosphorus-containing modified polypropylene fiber and 5 g of DOPO-modified oxidized carbon fiber, stir and mix evenly, pour the mixture into a mold, and press it in a plastic compression molding machine, wherein the pressure is 0.25 MPa, and the pressurization time is 28 min. After the pressing is completed, place it at room temperature and maintain the pressure for 20 h, dry it, and mold it to obtain an impact-resistant gypsum board.

[0035] Example 3

[0036] (1) Add 6 g of 4-vinylphenol to tetrahydrofuran solvent, stir and disperse, then add 3 g of hexachlorocyclotriphosphazene, stir and mix evenly, heat to 60°C, reflux for 72 hours, and after the reaction is completed, wash and dry to obtain an intermediate.

[0037] (2) Under nitrogen conditions, 20 g of polypropylene fiber was added to methanol solvent and stirred to disperse. Then, 25 g of the intermediate and 0.4 g of benzoyl peroxide were added thereto and stirred evenly. The temperature was raised to 85 °C and the reaction was carried out for 12 h. After the reaction was completed, the mixture was cooled to room temperature, washed with acetone, and dried to obtain phosphorus-containing modified polypropylene fiber.

[0038] (3) Under nitrogen conditions, 10 g of DOPO and 6 g of trimethoxyvinylsilane were added to a chloroform solvent and stirred for dispersion. Then, 0.07 g of azobisisobutyronitrile was added thereto and the mixture was reacted at 85 °C for 16 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain phosphorus-containing silane.

[0039] (4) Add 20 g of oxidized carbon fiber to ethanol solvent and disperse it ultrasonically. Then add 10% hydrochloric acid to adjust the pH to 3. Then add 20 g of phosphorus-containing silane and react at 70°C for 48 hours. After the reaction is completed, wash with deionized water and dry to obtain DOPO-modified oxidized carbon fiber.

[0040] (5) Add 100 g of gypsum powder and 0.1 g of gypsum retarder to 60 g of deionized water, stir and disperse, then add 10 g of phosphorus-modified polypropylene fiber and 10 g of DOPO-modified oxidized carbon fiber, stir and mix evenly, pour the mixture into a mold, and press it in a plastic compression molding machine, wherein the pressure is 0.3 MPa and the pressurization time is 20 min. After the pressing is completed, place it at room temperature and maintain the pressure for 12 h, dry it, and form it to obtain an impact-resistant gypsum board.

[0041] Example 4

[0042] (1) Add 7 g of 4-vinylphenol to tetrahydrofuran solvent, stir and disperse, then add 3 g of hexachlorocyclotriphosphazene, stir and mix evenly, heat to 65°C, reflux for 48 hours, and after the reaction is completed, wash and dry to obtain an intermediate.

[0043] (2) Under nitrogen conditions, 20 g of polypropylene fiber was added to methanol solvent and stirred to disperse. Then, 40 g of the intermediate and 1 g of benzoyl peroxide were added thereto and stirred evenly. The temperature was raised to 80 °C and the reaction was carried out for 10 h. After the reaction was completed, the mixture was cooled to room temperature, washed with acetone, and dried to obtain phosphorus-containing modified polypropylene fiber.

[0044] (3) Under nitrogen conditions, 10 g of DOPO and 8 g of trimethoxyvinylsilane were added to a chloroform solvent and stirred for dispersion. Then, 0.08 g of azobisisobutyronitrile was added thereto and the mixture was reacted at 75 °C for 24 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain phosphorus-containing silane.

[0045] (4) Add 20 g of oxidized carbon fiber to ethanol solvent and disperse it ultrasonically. Then add 10% hydrochloric acid to adjust the pH to 4. Then add 30 g of phosphorus-containing silane and react at 80°C for 24 hours. After the reaction is completed, wash with deionized water and dry to obtain DOPO-modified oxidized carbon fiber.

[0046] (5) Add 100 g of gypsum powder and 0.05 g of gypsum retarder to 80 g of deionized water, stir and disperse, then add 15 g of phosphorus-modified polypropylene fiber and 15 g of DOPO-modified oxidized carbon fiber, stir and mix evenly, pour the mixture into a mold, and press it in a plastic compression molding machine at a pressure of 0.3 MPa for 25 min. After the pressing is completed, place it at room temperature for 24 h, dry it, and form it to obtain an impact-resistant gypsum board.

[0047] Example 5

[0048] (1) Add 6 g of 4-vinylphenol to tetrahydrofuran solvent, stir and disperse, then add 3 g of hexachlorocyclotriphosphazene, stir and mix evenly, heat to 65°C, reflux for 48 hours, and after the reaction is completed, wash and dry to obtain an intermediate.

[0049] (2) Under nitrogen conditions, 20 g of polypropylene fiber was added to methanol solvent and stirred to disperse. Then, 20 g of the intermediate and 0.5 g of benzoyl peroxide were added thereto and stirred evenly. The temperature was raised to 90 °C and the reaction was carried out for 6 h. After the reaction was completed, the mixture was cooled to room temperature, washed with acetone, and dried to obtain phosphorus-containing modified polypropylene fiber.

[0050] (3) Under nitrogen conditions, 10 g of DOPO and 5 g of trimethoxyvinylsilane were added to chloroform solvent, stirred and dispersed, and then 0.1 g of azobisisobutyronitrile was added thereto. The reaction was carried out at 80°C for 12 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain phosphorus-containing silane.

[0051] (4) Add 20 g of oxidized carbon fiber to ethanol solvent and disperse it ultrasonically. Then add 10% hydrochloric acid to adjust the pH to 3. Then add 16 g of phosphorus-containing silane and react at 60°C for 20 h. After the reaction, wash with deionized water and dry to obtain DOPO-modified oxidized carbon fiber.

[0052] (5) Add 100 g of gypsum powder and 0.1 g of gypsum retarder to 70 g of deionized water, stir and disperse, then add 20 g of phosphorus-containing modified polypropylene fiber and 20 g of DOPO-modified oxidized carbon fiber, stir and mix evenly, pour the mixture into a mold, and press it in a plastic compression molding machine, wherein the pressure is 0.2 MPa and the pressurization time is 30 min. After the pressing is completed, place it at room temperature for 24 h, dry it, and form it to obtain an impact-resistant gypsum board.

[0053] Comparative Example 1

[0054] The difference between this comparative example and Example 1 is that in step (5), no phosphorus-containing modified polypropylene fiber is contained.

[0055] Comparative Example 2

[0056] The difference between this comparative example and Example 1 is that in step (5), DOPO-modified oxidized carbon fiber is not contained.

[0057] Use an electronic universal testing machine to test the compressive strength and flexural strength of the gypsum board.

[0058]

[0059] It can be seen from the table that the gypsum board prepared by the present invention has good flexural strength and compressive strength.

[0060] Refer to GB / T9775-2008 to test the fire stability of gypsum board.

[0061]

[0062] It can be seen from the table that the gypsum board prepared by the present invention has good fire stability.

[0063] The present invention uses the above embodiments to illustrate the impact-resistant gypsum board and the preparation method thereof, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An impact-resistant gypsum board, characterized in that: The impact-resistant gypsum board comprises the following components by weight: 100 parts of gypsum powder, 0.05-0.1 parts of gypsum retarder, 60-80 parts of deionized water, 1-20 parts of phosphorus-modified polypropylene fiber, and 1-20 parts of DOPO-modified oxidized carbon fiber; Wherein, the preparation method of the impact-resistant gypsum board is: Add gypsum powder and gypsum retarder to deionized water, stir and disperse, then add phosphorus-modified polypropylene fiber and DOPO-modified oxidized carbon fiber, stir and mix evenly, pour the mixture into a mold, and press in a plastic compression molding machine, wherein the pressure is 0.2-0.3MPa, the pressurization time is 20-30min, after the pressing is completed, place it at room temperature for 12-24h, dry, and mold to obtain an impact-resistant gypsum board; The preparation method of the phosphorus-containing modified polypropylene fiber is: (1) Add 4-vinylphenol to tetrahydrofuran solvent, stir and disperse, then add hexachlorocyclotriphosphazene, stir and mix evenly, heat to 60-75°C, reflux for 40-80h, wash and dry after the reaction, and obtain an intermediate, whose structural formula is , the mass ratio of 4-vinylphenol to hexachlorocyclotriphosphazene is 180-240:100; (2) Under nitrogen conditions, adding polypropylene fiber to methanol solvent, stirring and dispersing, then adding intermediate and benzoyl peroxide thereto, stirring evenly, heating to 80-90° C., reacting for 6-12 hours, cooling to room temperature after the reaction, washing with acetone, and drying to obtain phosphorus-containing modified polypropylene fiber, wherein the mass ratio of the polypropylene fiber, intermediate, and benzoyl peroxide is 100:100-200:2-5; The preparation method of the DOPO-modified oxidized carbon fiber is as follows: S1. Under nitrogen conditions, DOPO and trimethoxyvinylsilane are added to a chloroform solvent, stirred and dispersed, and then azobisisobutyronitrile is added thereto, and the reaction is carried out at 75-85° C. for 12-24 hours. After the reaction is completed, the phosphorus-containing silane is obtained by vacuum distillation, wherein the mass ratio of DOPO, trimethoxyvinylsilane and azobisisobutyronitrile is 100:50-80:0.7-1; S2. Add oxidized carbon fiber to ethanol solvent, disperse by ultrasonic, add 10% hydrochloric acid to adjust the pH to 3-4, add phosphorus-containing silane to it, react at 60-80°C for 20-48h, wash with deionized water after the reaction, and dry to obtain DOPO-modified oxidized carbon fiber, wherein the mass ratio of oxidized carbon fiber to phosphorus-containing silane is 100:80-150.