Bio-based all-water foaming degradable packaging material and preparation method thereof

By using raw materials such as hydroxyethyl chitosan and modified polyester to prepare a polymer cross-linked structure, the problem of insufficient water resistance and mechanical properties of all-bio-based all-water foam packaging materials has been solved, achieving a tougher and more durable product. packaging materials and have made significant progress in environmental friendliness and degradability.

CN118791689AInactive Publication Date: 2024-10-18HUIZHOU JIASHENG PACKING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411058977.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fully bio-based fully water-foamed degradable packaging materials have insufficient water resistance and mechanical properties, making it difficult to meet the application needs of packaging materials in food, pharmaceuticals and other fields.

Method used

It adopts a combined formula of hydroxyethyl chitosan, modified polyester, foaming agent, foam stabilizer and catalyst. Through the modifier, 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde , polyether polyol and other raw materials are used to prepare modified polyester, and the prepolymer is obtained through mechanical stirring and heat treatment, and then reacts with modifiers and compatibilizers to form a polymer cross-linked structure to improve the mechanical properties and degradability of the material. sex.

Benefits of technology

It significantly improves the mechanical properties and water resistance of packaging materials, extends the shelf life, and achieves efficient biodegradation in the natural environment, reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004977230500000091
    Figure BDA0004977230500000091
Patent Text Reader

Abstract

The invention discloses a bio-based all-water foaming degradable packaging material and a preparation method thereof. The packaging material is prepared from hydroxyethyl chitosan and modified polyester. The preparation method comprises the following steps: firstly, carrying out reaction on hydroxyl in polycaprolactone glycol, 2-ethyl-4, 6-dihydroxy-3-methylbenzaldehyde and isocyanato in a compatilizer to obtain a polyester prepolymer, and carrying out reaction on the polyester prepolymer serving as a cross-linking agent and hydroxyl in a modifier to obtain modified polyester; and finally, foaming the modified polyester and hydroxyethyl chitosan under the action of a foaming agent and other auxiliaries to prepare the packaging material. Compared with the prior art, the packaging material prepared by the invention has the advantages of good water resistance, good mechanical properties and degradability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of packaging materials, and in particular to a bio-based fully water-foamed degradable packaging material and a preparation method thereof. Background Art

[0002] As global environmental pollution and resource depletion become increasingly serious, people are paying more and more attention to environmental protection and sustainable development. In the packaging industry, traditional petroleum-based plastic packaging materials have caused serious pollution to the environment due to their difficulty in degradation.

[0003] Therefore, the development of an environmentally friendly and degradable packaging material has become an urgent problem that needs to be solved. Bio-based fully water-foamed degradable packaging material came into being. It is a new type of environmentally friendly packaging material, mainly made of bio-based materials, with good degradability and biocompatibility. Compared with traditional petroleum-based plastic packaging materials, bio-based fully water-foamed degradable packaging materials have many advantages, such as: degradability, bio-based raw materials, safety, processing performance, etc. Due to the many advantages of bio-based fully water-foamed degradable packaging materials, it is widely used in the packaging of food, medicine, cosmetics and other products, which can not only reduce environmental pollution, but also improve the safety and quality of products.

[0004] CN114685920B discloses a degradable packaging material and a synthesis method thereof, wherein o-nitrobenzyl alcoholized caged silsesquioxane monomer P3 is synthesized by hydrosilylation of o-nitrobenzyl alcohol functional monomer P1 and alkenylation of phenyl caged silsesquioxane monomer P2, and o-nitrobenzyl alcoholized caged silsesquioxane monomer P3 is subjected to a dehydration condensation reaction with 2-[dodecylthio (thiocarbonyl)thio]-2-methylpropionic acid to generate a reversible addition-fragmentation chain transfer monomer P4, which is used as a chain transfer agent, and 4-hydroxystyrene and 4-vinylaniline undergo a reversible addition-fragmentation chain transfer polymerization reaction to generate hydroxylated amino styrene microspheres, and polyvinyl alcohol is modified with the microspheres to obtain a polyvinyl alcohol-based degradable packaging material having excellent mechanical properties, water resistance, chemical degradation, and optical degradation. However, the packaging material raw material prepared by the method uses chemically synthesized substances, which has a great environmental pollution.

[0005] CN113442533A discloses a degradable polymer composite material, a preparation method and a food packaging film, comprising: an outer layer, wherein the outer layer is a mixture of polypropylene and polyhydroxyheptanoate; a filling layer, wherein the filling layer is a mixture of polyvinyl alcohol, sodium carboxymethyl cellulose and polystyrene; and an inner layer, wherein the inner layer is a mixture of polyethylene, polyhydroxyheptanoate and vinyl acetate; wherein the outer layer, the filling layer and the inner layer all exhibit a biodegradation rate as measured according to the ASTMD5338-92 standard. The invention uses polyvinyl alcohol and sodium carboxymethyl cellulose as the main components to make an intermediate layer sheet of a composite material, and then coats a polypropylene inner layer and a polyethylene outer layer, thereby solving the water resistance of the material and effectively reducing the cost of the material. By adding 40-55% of polyhydroxyheptanoate to the inner and outer films, the film has excellent biodegradability and maintains the original physical properties. However, the packaging film prepared by this method has poor mechanical properties and is prone to rupture and other problems. Summary of the invention

[0006] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to improve the water resistance and mechanical properties of the all-biobased, all-water-foamed, degradable packaging material.

[0007] To achieve the above-mentioned purpose, the present invention provides a bio-based fully water-foamed degradable packaging material, which comprises the following weight components, in parts by weight: 2-8 parts of hydroxyethyl deacetylated chitosan, 20-40 parts of modified polyester, 2-20 parts of foaming agent, 0.1-3 parts of foam stabilizer, and 0.1-2 parts of catalyst. The modified polyester is prepared from the modifier, 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde, a degradable polymer, and a polyether polyol.

[0008] Preferably, the preparation method of the modified polyester comprises the following steps:

[0009] S1. Dissolve polyether polyol, degradable polymer, 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde and compatibilizer in a solvent, stir mechanically, heat to 70-85° C. under nitrogen, continue mechanical stirring for 2-4 hours, and then remove the solvent by vacuum rotary evaporation to obtain prepolymer A;

[0010] S2. The modifier and the prepolymer A obtained in S1 are mixed at 500-800 rpm for 5-15 min, and then mixed at 100-200 rpm for 1-2 h at 80-95° C. under nitrogen conditions to obtain modified polyester.

[0011] More preferably, the method for preparing the modified polyester comprises the following steps, in parts by weight:

[0012] S1. Dissolve 10-40 parts of polyether polyol, 5-10 parts of degradable polymer, 0.1-2 parts of 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde and 1-7 parts of compatibilizer in 8-20 parts of solvent, stir mechanically, heat to 70-85° C. under nitrogen, continue mechanical stirring for 2-4 hours, and then remove the solvent by vacuum rotary evaporation to obtain prepolymer A;

[0013] S2. Mix 1-6 parts of prepolymer A obtained from modifier S1 at 500-800 rpm for 5-15 min, and then mix at 100-200 rpm for 1-2 h at 80-95° C. under nitrogen to obtain modified polyester.

[0014] Preferably, the modifier is any one of lignin, xylitol, cyclodextrin, and 2-hydroxy-3-mercaptosuccinic acid.

[0015] More preferably, the modifier is 2-hydroxy-3-mercaptosuccinic acid.

[0016] Preferably, the compatibilizer is any one of m-phenylene diisocyanate, dimethyl diphenyl diisocyanate, and benzene-1,2,4,5-tetrafluoro-3,6-diisocyanate.

[0017] Preferably, the degradable polymer is any one of polycaprolactone diol, polylactic acid and polycaprolactone diol.

[0018] Preferably, the catalyst is a mixture of stannous isooctanoate and triethylenediamine.

[0019] A method for preparing a bio-based fully water-foamed degradable packaging material comprises the following steps, measured in parts by weight:

[0020] Step 1, weigh 2-8 parts of hydroxyethyl deacetylated chitosan and 20-40 parts of modified polyester, knead and mix them evenly to obtain a polymer;

[0021] Step 2: Evenly mix 2-20 parts of foaming agent, 0.1-3 parts of foam stabilizer, 0.1-2 parts of catalyst and the polymer in step 1, pour into a mold for foaming, solidify after foaming, cool and demould to obtain a bio-based fully water-foamed degradable packaging material.

[0022] In this recipe, the ingredients and their functions are as follows:

[0023] Hydroxyethyl chitosan: Hydroxyethyl chitosan is a chitosan derivative and a natural polysaccharide. It has the characteristics of strong antimicrobial activity, good biocompatibility and excellent biodegradability. Secondly, hydroxyethyl chitosan has good mechanical properties, which can enhance the structural stability of packaging materials and make them tougher and more durable. In addition, hydroxyethyl chitosan also has excellent gas barrier properties, which can effectively prevent the penetration of oxygen and moisture, thereby protecting the items in the package and extending their shelf life. Hydroxyethyl chitosan contains amino functional groups and hydroxyl functional groups, wherein the amino functional groups can react with the aldehyde functional groups contained in the prepared modified polyester to prepare a bio-based degradable polymer.

[0024] Modifier: The modifier contains a hydroxyl functional group. As one of the raw materials for synthesizing modified polyester, the hydroxyl functional group in the modifier can react with the aldehyde functional group contained in the polymer that reacts with each other among polycaprolactone diol, 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde and the compatibilizer, thereby grafting the modifier onto the polymer to prepare the modified polyester.

[0025] 2-Ethyl-4,6-dihydroxy-3-methylbenzaldehyde: The aldehyde functional group contained in 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde can participate in the polymerization reaction between the hydroxyl functional group of polycaprolactone diol and the isocyanate functional group of the compatibilizer to form a stable chemical bond to obtain a polymer compound, thereby enhancing the molecular structure of the modified polyester.

[0026] Polycaprolactone diol: Polycaprolactone diol has good biodegradability and can be decomposed by microorganisms in the natural environment, reducing environmental pollution. In the preparation process of packaging materials, the glass transition temperature of polycaprolactone diol is extremely low, and its permeability is better than other polyester materials at room temperature. In addition, the melting point of polycaprolactone diol is relatively low, so its flexibility and processability are good. Although the blending of modifiers with aliphatic modified polyesters can make up for some of the shortcomings of single packaging materials, they often face many problems such as interface incompatibility. The use of compatibilizers containing isocyanate functional groups can play a huge role in improving the separation between the two-phase interface of the modifier and the modified polyester composite material. When there are two or more isocyanate groups in a molecule of compatibilizer, a special "interface cross-linking layer" will be formed, which can reduce the separation tendency between the modifier and polycaprolactone diol, the gap disappears, and the interaction in the composite material increases, thereby enhancing the performance of the composite material. In addition, when polycaprolactone diol is selected as the soft segment, physical cross-linking will also occur due to the similar structure, and the interface compatibility will also become better.

[0027] Compatibilizer: As a raw material for synthesizing modified polyester, compatibilizer contains isocyanate functional groups, which can be cross-linked with the hydroxyl functional groups contained in polycaprolactone diol and the aldehyde functional groups contained in 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde to obtain a high molecular polymer. The obtained high molecular polymer is then cross-linked with the modifier to obtain the modified polyester. Among them, the use of a compatibilizer can reduce the separation tendency between the modifier and polycaprolactone diol, allowing the two to be better integrated, thereby increasing the density of the modified polyester.

[0028] Foaming agent: Water is used as a foaming agent, that is, the gas CO2 generated by the reaction of water and isocyanate is used for foaming. Water is an ideal substitute for chlorofluorocarbons. The polyurethane foam plastic produced has no toxic side effects, has zero potential for depletion of the ozone layer, and will not cause a greenhouse effect.

[0029] Polyether polyol: Polyether polyol is one of the indispensable main raw materials in the synthesis process of modified polyester materials. The structure of polyether polyol has a great influence on the structure of polyurethane foam. The hydroxyl value and functionality of polyol directly affect the crosslinking degree of polyurethane foam.

[0030] Foam stabilizer: Foam stabilizer is also called foam leveler. It is an indispensable component in the foaming process of preparing modified polyester. It can increase the mutual solubility between the components in the production process, play the role of emulsification, nucleation and stabilization of foam cells. It plays the role of stabilizing bubbles in the foam molding process, so that the foam plastics have uniform pore size, high closed cell rate, good thermal insulation effect, etc.

[0031] Catalyst: Catalysts can promote chemical reactions, increase reaction rates, and make the synthesis of modified polyesters more efficient.

[0032] N,N-dimethylformamide: As a solvent, N,N-dimethylformamide has good solubility and can effectively dissolve various raw materials used in the preparation of modified polyester.

[0033] Beneficial effects of the present invention:

[0034] 1. Compared with the prior art, the present invention obtains a polyester prepolymer with an isocyanate terminal group by reacting the hydroxyl functional group contained in polycaprolactone diol, the aldehyde functional group contained in 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde, and the isocyanate contained in the compatibilizer, and then reacts the polyester prepolymer with the hydroxyl functional group contained in the modifier to obtain a modified polyester, and finally cross-links the modified polyester with the amino group in hydroxyethyl deacetylated chitosan to obtain a degradable packaging material.

[0035] 2. Compared with the prior art, the present invention obtains a polyester prepolymer by activating the terminal group to isocyanate, and introduces it into the modifier as a cross-linking agent to obtain a modified polyester after the reaction. At the same time, by optimizing the segment structure of the modified polyester and adding new functional groups, a double-cross-linked modified biodegradable film is obtained, thereby improving the degradability of the packaging material. DETAILED DESCRIPTION

[0036] Parameters for specific chemical substances used, sources.

[0037] 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde, CAS No.: 63521-10-8.

[0038] Benzene,1,2,4,5-tetrafluoro-3,6-diisocyanato-, CAS No.: 16346-58-0.

[0039] 2-Hydroxy-3-mercaptobutanedioic acid, CAS No.: 16023-31-7.

[0040] Polycaprolactone diol, CAS No. 36890-68-3, average molecular weight about 2000, source: Shanghai Aladdin Biochemical Technology Co., Ltd.

[0041] The starch in the examples is commercially available corn starch.

[0042] Polyether polyol, product number E762212, viscosity (25°C): 260-380 mPa·s, hydroxyl value: 335 mgKOH / g, source: Shanghai MacLean Biochemical Technology Co., Ltd.

[0043] Dimethyl silicone oil, CAS No. 63148-62-9, product No. 767026, viscosity (25°C): 130±10mPa.s, source: Shanghai MacLean Biochemical Technology Co., Ltd.

[0044] Example 1

[0045] A method for preparing a bio-based fully water-foamed degradable packaging material comprises the following steps:

[0046] Step 1, weigh 5 kg of hydroxyethyl deacetylated chitosan and 30 kg of modified polyester, add them into a twin-screw extruder equipped with a mixing function, set the speed to 35 rpm, the temperature to 160° C., the time to 25 min, and extrude to obtain a polymer;

[0047] Step 2: Stir a mixture of 3 kg of water, 1 kg of dimethyl silicone oil, 0.2 kg of stannous isooctanoate and 0.3 kg of triethylenediamine with the polymer in step 1 at 3000 rpm for 50 seconds, pour into a mold and stir at 3000 rpm for 15 seconds, then foam for 2 minutes, and after foaming, cure at 25°C for 24 hours, and finally cool and demold to obtain a bio-based fully water-foamable degradable packaging material.

[0048] Wherein, the preparation method of the modified polyester comprises the following steps:

[0049] S1. Dissolve 30 g of polyether polyol, 10 g of polycaprolactone diol, 0.6 g of 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde and 3 g of benzene-1,2,4,5-tetrafluoro-3,6-diisocyanate in 15 mL of N,N-dimethylformamide, stir at 200 rpm for 20 min, heat to 80° C. under nitrogen, continue mechanical stirring for 3 h, and then evaporate at 2.05 KPa and 90° C. for 2 h to remove the solvent to obtain prepolymer A;

[0050] S2. 5 g of 2-hydroxy-3-mercaptosuccinic acid and the prepolymer A obtained in S1 were mixed at 700 rpm for 10 min, and then mixed at 160 rpm for 1.5 h at 85° C. under nitrogen conditions to obtain a modified polyester.

[0051] Example 2

[0052] The difference between Example 2 of the present application and Example 1 is that the 2-hydroxy-3-mercaptosuccinic acid in Example 1 is replaced by lignin.

[0053] Example 3

[0054] The difference between Example 3 of the present application and Example 1 is that the 2-hydroxy-3-mercaptosuccinic acid in Example 1 is replaced by xylitol.

[0055] Example 4

[0056] The difference between Example 4 of the present application and Example 1 is that the 2-hydroxy-3-mercaptosuccinic acid in Example 1 is replaced by α-cyclodextrin.

[0057] Example 5

[0058] The difference between Example 5 of the present application and Example 1 is that the benzene-1,2,4,5-tetrafluoro-3,6-diisocyanate in Example 1 is replaced by isophenylene diisocyanate.

[0059] Example 6

[0060] The difference between Example 6 of the present application and Example 1 is that the benzene-1,2,4,5-tetrafluoro-3,6-diisocyanate in Example 1 is replaced by dimethylbiphenyl diisocyanate.

[0061] Comparative Example 1

[0062] The difference between Comparative Example 1 and Example 1 is that the 2-hydroxy-3-mercaptosuccinic acid in Example 1 is replaced by starch.

[0063] Comparative Example 2

[0064] The difference between Comparative Example 2 and Example 1 is that the benzene-1,2,4,5-tetrafluoro-3,6-diisocyanate in Example 1 is replaced by isophorone diisocyanate.

[0065] Test Case

[0066] Test of mechanical properties: According to GB / T 1040.2-2022 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics", the standard strip samples of packaging materials prepared in Examples 1-6 and Comparative Examples 1-2 with a size of 150 mm × 10 mm × 0.4 mm were placed under constant temperature and humidity conditions for 5 days, and then tensile tests were carried out with a universal electronic tensile testing machine at a tensile rate of 10 mm / min. The tensile strength and elongation at break were tested, and the average value of the 5 samples was taken.

[0067] Degradability test: The degradation rate test is carried out according to ASTM D5338-92, where the culture time is 45 days; the compost material used for the test inoculation is required to meet the following conditions: ash content is less than 70%, pH value is 7-8, 50mg-150mg carbon dioxide can be produced per gram of volatile solids in the first 10 days of the test, and the carbon-nitrogen ratio is between 10-20; the culture temperature is: 35℃ on the first day, 50℃ from the second to the 28th day, and 35℃ from the 29th to the 45th day. The degradation rate is the percentage of the carbon element amount converted into CO2 of the sample under the above test conditions and the sample weight. The calculation formula is: D=Wco2×12 / 44×100%, Wco2=Gco2 / Gsample, where D is the degradation rate, %; Wco2 is the cumulative amount of CO2 produced by the unit weight of the sample due to degradation, g / g; Gco2 is the cumulative amount, g; Gsample is the sample weight, g.

[0068] Water resistance: Water resistance test: The static contact angle of the packaging materials prepared in Examples 1-6 and Comparative Examples 1-2 to water is expressed by a contact angle meter. The size of the water droplet is 5 μL. The average value is taken after 3 measurements. The test results are shown in Table 1:

[0069] Table 1 Mechanical properties and water resistance test

[0070]

[0071] By observing the test examples and the test data results in Table 1, it can be found that the mechanical properties, water resistance and degradation properties of the bio-based fully water-foamed degradable packaging material prepared in Example 1 are the best.

[0072] Comparing the data of Examples 1-4 and Comparative Example 1, it is found that the differences between the data are quite obvious, and the reason may be that different modifiers are used. First, the hydroxyl functional group contained in the polycaprolactone diol, the aldehyde functional group contained in the 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde, and the isocyanate contained in the compatibilizer are reacted to obtain an isocyanate polyester prepolymer with an end group. The role of the modifier is to cross-link and modify the modified polyester to increase the physical or chemical properties such as biocompatibility and mechanical properties of the modified polyester. The modified polyester is prepared by reacting the isocyanate polyester prepolymer with an end group as a cross-linking agent with a modifier containing a hydroxyl functional group. The polyester prepolymer generated by the low molecular weight polycaprolactone diol chain increases the content of the isocyanate group, so more carbamate bonds are generated between the interface of the polyester prepolymer and the modifier, thereby promoting the compatibility of the modifier and the polyester prepolymer. After the compatibility is improved, the degree of cross-linking is better, the dispersibility of the modifier in the modified polyester matrix is ​​relatively good, and the mechanical strength of the prepared modified polyester polymer will be higher, so it has higher tensile strength and Young's modulus, and thus exhibits excellent mechanical properties.

[0073] In addition to the hydroxyl functional group, the modifier in Example 1 also contains a thiol functional group. When the isocyanate functional group contained in the compatibilizer is subjected to a chain extension reaction with a dihydroxy compound containing a thiol functional group, a thiol-isocyanate reaction occurs, which is a special chemical reaction that can form a thiourethane bond. This reaction usually occurs under mild conditions, and the thiol reacts with the isocyanate to form a thiourethane structure. This stable thiourethane structure has a resistance to the hydrolysis and degradation pathway of the packaging material. In the prepared modified polyester, the dynamic covalent bonds in the cross-linked network have a high degree of uniformity, and bond exchange and bond dissociation can occur reversibly without affecting the degree of crosslinking, so that the modified polyester can be recycled and reprocessed, and exhibits more excellent thermal stability. This stable molecular structure also helps to improve tensile strength and elongation at break, because it has stronger intermolecular interactions that can resist external tensile forces. Because the modifier used in Example 1 also contains a thiol functional group and can generate a dynamic thiopolyurethane structure, the packaging material prepared in Example 1 has better mechanical strength and thermal stability than the modifiers containing only hydroxyl functional groups in Examples 2-4.

[0074] Comparing the data in the table of Example 1, Example 5-6 and Comparative Example 2, it is found that the data are all different, and the reason for these differences may be that different compatibilizers are used. Compatibilizer provides isocyanate functional group, which serves as the raw material for preparing modified polyester. The hard segment constituting modified polyester provides hard and brittle rigidity, and can react with the alcohol hydroxyl group in polycaprolactone diol to generate carbamate. The compatibilizer in Example 1 contains fluorine atoms in addition to isocyanate functional group. Fluorine atoms have many advantages such as small atomic radius, low surface energy, strong electronegativity, etc. The carbon-fluorine bond with high bond energy and the carbon-fluorine chain with strong rigidity make organic fluorine compounds become good modified substances for modified polyester. Fluorine polarizability is low, and molecular dipole moment is small, so that organic fluorine materials can show excellent water resistance. The compatibilizer acts as the hard segment of the high molecular weight polymer, and the alcoholic hydroxyl group in the polycaprolactone diol directly reacts with the fluorine-containing isocyanate, so that the fluorine atom can be introduced into the modified polyester, thereby making the packaging material prepared from the modified polyester have excellent water resistance. Because the compatibilizer in Example 1 contains fluorine atoms, while the compatibilizers in Examples 5-6 and Comparative Example 2 do not contain fluorine atoms, and fluorine can be introduced into the modified polyester to make the material hydrophobic, the packaging material prepared in Example 1 has better water resistance.

Claims

1. A bio-based fully water-foamed degradable packaging material, characterized in that: The invention comprises the following components in parts by weight: 2-8 parts of hydroxyethyl deacetylated chitosan, 20-40 parts of modified polyester, 2-20 parts of foaming agent, 0.1-3 parts of foam stabilizer and 0.1-2 parts of catalyst. The modified polyester is prepared from the modifier, 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde, a degradable polymer, a compatibilizer and a polyether polyol.

2. The bio-based fully water-foamed degradable packaging material according to claim 1, characterized in that: The preparation method of the modified polyester comprises the following steps: S1. Dissolve polyether polyol, degradable polymer, 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde and compatibilizer in a solvent, stir mechanically, heat to 70-85° C. under nitrogen, continue mechanical stirring for 2-4 hours, and then remove the solvent by vacuum rotary evaporation to obtain prepolymer A; S2. The modifier and the prepolymer A obtained in S1 are mixed at 500-800 rpm for 5-15 min, and then mixed at 100-200 rpm for 1-2 h at 80-95° C. under nitrogen conditions to obtain modified polyester.

3. The bio-based fully water-foamed degradable packaging material according to claim 1, characterized in that: The preparation method of the modified polyester comprises the following steps, measured in parts by weight: S1. Dissolve 10-40 parts of polyether polyol, 5-10 parts of degradable polymer, 0.1-2 parts of 2-ethyl-4,6-dihydroxy-3-methylbenzaldehyde and 1-7 parts of compatibilizer in 8-20 parts of solvent, stir mechanically, heat to 70-85° C. under nitrogen, continue mechanical stirring for 2-4 hours, and then remove the solvent by vacuum rotary evaporation to obtain prepolymer A; S2. Mix 1-6 parts of the modifier and the prepolymer A obtained in S1 at 500-800 rpm for 5-15 min, and then mix at 100-200 rpm for 1-2 h at 80-95° C. under nitrogen to obtain a modified polyester.

4. The bio-based fully water-foamed degradable packaging material according to claim 1, characterized in that: The modifier is any one of lignin, xylitol, cyclodextrin and 2-hydroxy-3-mercaptosuccinic acid.

5. The bio-based fully water-foamable degradable packaging material according to claim 4, characterized in that: The modifier is 2-hydroxy-3-mercaptosuccinic acid.

6. The bio-based fully water-foamed degradable packaging material according to claim 1, characterized in that: The compatibilizer is any one of m-phenylene diisocyanate, dimethyl biphenyl diisocyanate, and benzene-1,2,4,5-tetrafluoro-3,6-diisocyanate.

7. The bio-based fully water-foamed degradable packaging material according to claim 1, characterized in that: The degradable polymer is any one of polycaprolactone diol, polylactic acid, and polybutylene terephthalate-adipate.

8. The bio-based fully water-foamed degradable packaging material according to claim 1, characterized in that: The catalyst is a mixture of stannous isooctanoate and triethylenediamine.

9. The method for preparing the bio-based fully water-foamable degradable packaging material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps, in parts by weight: Step 1, weigh 2-8 parts of hydroxyethyl deacetylated chitosan and 20-40 parts of modified polyester, knead and mix them evenly to obtain a polymer; Step 2: Evenly mix 2-20 parts of foaming agent, 0.1-3 parts of foam stabilizer, 0.1-2 parts of catalyst and the polymer in step 1, pour into a mold for foaming, solidify after foaming, cool and demould to obtain a bio-based fully water-foamed degradable packaging material.

Citation Information

Patent Citations

  • Chitosan-polyurethane composite rigid closed-cell foam material and preparation method thereof

    CN101781396A

  • Biodegradable polyurethane composite material for packaging and preparation method thereof

    CN110938188A

  • Bio-based polyurethane foam and preparation method thereof

    CN112646112A

  • All-water-foaming polyurethane microporous elastomer double-peak damping material based on molecular design and preparation method of all-water-foaming polyurethane microporous elastomer double-peak damping material

    CN116333260A

  • Composition for preparing a biodegradable polyurethane- based foam and a biodegradable polyurethane foam

    US20090253816A1