Titanium nitride composite slurry, coating as well as preparation method and application of titanium nitride composite slurry
By combining modified titanium nitride powder with silane coupling agent and dispersant, a titanium nitride composite slurry with high infrared blocking rate and good dispersion effect is prepared, which solves the problem of poor infrared blocking rate of existing titanium nitride slurries. problem, suitable for a variety of insulation applications.
Patent Information
- Application Number
- CN202411043917.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-18
AI Technical Summary
The existing titanium nitride slurry has poor infrared blocking rate and poor dispersion effect, resulting in low blocking efficiency.
Modified titanium nitride powder is combined with silane coupling agent and dispersant to prepare titanium nitride composite slurry through specific mass percentage and treatment methods to ensure its uniformity and stability of dispersion, using non-polar solvents and fatty acid methyl Ester is used as a solvent, and the average particle size is controlled at <100nm to improve the infrared blocking effect.
The prepared titanium nitride composite slurry has high infrared blocking rate and good visible light transmittance, is evenly dispersed, and is suitable for multiple application scenarios, such as car film and building glass window film. The preparation process is simple and easy to operate, and is suitable for industrial production. .
Smart Images

Figure CN118791901A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a titanium nitride composite slurry, a coating and a preparation method and application thereof. Background Art
[0002] In recent years, due to the large amount of greenhouse gas emissions (such as carbon dioxide, methane, etc.) caused by human activities, the average temperature of the earth has been rising year by year, which is manifested as the trend of global warming, which is particularly obvious in summer. The strong solar radiation in summer causes the temperature of closed environments such as indoors and cars to continue to rise, resulting in an increasing demand for thermal insulation functions in the automotive and architectural glass industries. Therefore, the development of new high thermal insulation materials has a very broad application prospect in the fields of construction and industry.
[0003] Nano thermal insulation slurry is a new type of coating that absorbs and shields near-infrared light and ultraviolet light. It can increase the thermal insulation effect on architectural and industrial glass structures to achieve the goal of energy saving and consumption reduction. In recent years, with the continuous deepening of research, various inorganic powders such as indium tin oxide (ITO), antimony tin oxide (ATO), cesium tungsten bronze (CWO) and lanthanum hexaboride (LaB6) are widely used in the field of high thermal insulation slurry. However, these materials still have some obvious defects: the powder is unevenly dispersed in the slurry, it is easy to agglomerate, and the barrier efficiency is reduced.
[0004] Titanium nitride (TiN) refers to a transition metal nitride, which is a mixed bond crystal composed of metallic bonds, ionic bonds and covalent bonds. It has the characteristics of high melting point, high hardness, wear resistance, corrosion resistance, good thermal conductivity and electrical conductivity, excellent infrared reflection performance, etc. The slurry made of titanium nitride powder has a high dispersion system, is not easy to agglomerate, and has high infrared blocking efficiency, which can greatly reduce energy consumption, but it still has some defects, such as poor dispersion effect of slurry and poor infrared blocking effect. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defect of poor infrared blocking effect of titanium nitride slurry in the prior art, and provide a titanium nitride composite slurry, coating and preparation method and application thereof. The titanium nitride composite slurry system of the present invention is stable, evenly dispersed and not easy to agglomerate. The coating prepared from the titanium nitride composite slurry has better infrared blocking rate, visible light transmittance and haze, and can be widely used in multiple scenarios.
[0006] The present invention solves the above technical problems through the following technical solutions.
[0007] The present invention provides a titanium nitride composite slurry, which comprises the following components in percentage by mass:
[0008] 10%-40% modified titanium nitride powder; 15%-60% dispersant; 20%-75% organic solvent B; the organic solvent B is a non-polar solvent and / or fatty acid methyl ester; the average particle size of the titanium nitride composite slurry is less than 100nm;
[0009] The modified titanium nitride powder is titanium nitride powder modified by a silane coupling agent;
[0010] The above mass percentages represent the percentage of the mass of each component to the total mass of the titanium nitride composite slurry.
[0011] In the present invention, the mass percentage of the modified titanium nitride powder is preferably 18%-38%, such as 20% or 35%; the above mass percentage represents the percentage of the mass of the modified titanium nitride powder to the total mass of the titanium nitride composite slurry.
[0012] In the present invention, the method for preparing the modified titanium nitride powder preferably comprises mixing a silane coupling agent and titanium nitride powder, and more preferably comprises mixing and reacting titanium nitride powder, a silane coupling agent and a solvent A.
[0013] The average particle size of the titanium nitride powder may be 20-100 nm, preferably 20-60 nm, such as 50 nm.
[0014] The mass percentage of the titanium nitride powder may be 10%-50%, preferably 20%-30%, for example 25%. The mass percentage indicates the mass percentage of the titanium nitride powder to the total mass of the titanium nitride powder, the silane coupling agent and the ethanol aqueous solution.
[0015] Wherein, the molecular formula of the silane coupling agent can be Y n SiX3, wherein n can be a natural number of 1-3, such as 1, 2 or 3. In the silane coupling agent, Y can include an acryloxy group, and preferably also includes one or more of a vinyl group, an allyl group, an alkyl group, a hydrogen group, an epoxy group and a mercapto group. The alkyl group can be a methyl group. X preferably includes one or more of a methoxy group, an ethoxy group, an acyloxy group, an aryloxy group and a tert-butyl peroxy group, such as a methoxy group.
[0016] In a preferred embodiment, the molecular formula of the silane coupling agent is Y1SiX3, where Y is an epoxy group and X is a methoxy group.
[0017] In a preferred embodiment, the molecular formula of the silane coupling agent is Y n SiX3, n is 1, Y is acryloyloxy and alkyl, and X is methoxy.
[0018] The silane coupling agent is preferably KH-560, KH-570, A-174, KBM-503 or SH-6030, for example, KH-560 or KH-570.
[0019] The mass percentage of the silane coupling agent may be 10%-30%, preferably 12%-25%, such as 12.5%. The mass percentage indicates the mass percentage of the silane coupling agent to the total mass of the titanium nitride powder, the silane coupling agent and the ethanol aqueous solution.
[0020] The molar ratio of the titanium nitride powder to the silane coupling agent may be (5-10):1, preferably (6-9):1, such as 7.6:1 or 8:1.
[0021] Wherein, the solvent A may be an ethanol aqueous solution. The mass percentage of the solvent A may be 40%-70%, preferably 50%-65%, for example 62.5%. The mass percentage indicates the mass percentage of the solvent A to the total mass of the titanium nitride powder, the silane coupling agent and the solvent A.
[0022] Wherein, in the solvent A, the mass percentage of the active ingredient may be 70%-90%, for example 80%.
[0023] The reaction temperature may be 60-90°C, such as 70 or 80°C.
[0024] The reaction time may be 1-4 hours, such as 2 or 3 hours.
[0025] Wherein, the reaction can be carried out in a water bath or an oil bath.
[0026] After the reaction, washing and drying steps are generally included. The washing operation can be conventional in the art, such as centrifugal washing with ultrapure water. The drying operation can be conventional in the art, such as drying in an oven. The drying temperature can be 50-100°C, such as 70°C. The drying time can be 12-36h, such as 20h.
[0027] In the present invention, the average particle size of the modified titanium nitride powder is preferably 50-70 nm, preferably 50-58 nm.
[0028] In the present invention, the mass percentage of the dispersant is preferably 20%-55%, such as 25%, 30%, 40% or 50%; the above mass percentage represents the mass percentage of the dispersant to the total mass of the titanium nitride composite slurry.
[0029] In the present invention, the type of the dispersant may be a copolymer containing an acidic group. The acidic group may be a conventional group in the art that can generate hydrogen ions during hydrolysis or ionization, such as a carboxyl group and / or a sulfonic acid group. The dispersant is preferably a carboxylate copolymer, more preferably a styrene maleic anhydride copolymer, such as TEGO Dispers 670.
[0030] In the present invention, the mass percentage of the organic solvent B is preferably 30%-70%, such as 35%, 40%, 50% or 70%; the above mass percentage represents the mass percentage of the organic solvent B to the total mass of the titanium nitride composite slurry.
[0031] In the present invention, the non-polar solvent may be benzene and its derivatives, preferably xylene.
[0032] In the present invention, the fatty acid methyl ester may be a fatty acid methyl ester having 1 to 3 carbon atoms, preferably methyl acetate.
[0033] In the present invention, the organic solvent B is preferably xylene and / or methyl acetate.
[0034] In the present invention, the average particle size of the titanium nitride composite slurry is preferably <98 nm, such as 94, 92, 84, 77, 48, 50, 51, 52 nm or 69 nm. The average particle size of the titanium nitride composite slurry refers to the average particle size of titanium nitride in the titanium nitride composite slurry system.
[0035] The present invention also provides a method for preparing a titanium nitride composite slurry, which comprises the following steps:
[0036] 10%-40% of modified titanium nitride powder, 15%-60% of dispersant and 20%-75% of organic solvent B are mixed; the organic solvent B is a non-polar solvent and / or fatty acid methyl ester; the average particle size of the titanium nitride composite slurry is less than 100nm; the above mass percentage represents the percentage of the mass of each component to the total mass of the titanium nitride composite slurry;
[0037] The modified titanium nitride powder is titanium nitride powder modified by a silane coupling agent.
[0038] In the present invention, the mass percentage of the modified titanium nitride powder is preferably 18%-38%, such as 20% or 35%; the above mass percentage represents the percentage of the mass of the modified titanium nitride powder to the total mass of the titanium nitride composite slurry.
[0039] In the present invention, the method for preparing the modified titanium nitride powder preferably comprises mixing a silane coupling agent and titanium nitride powder, and more preferably comprises mixing and reacting titanium nitride powder, a silane coupling agent and a solvent A.
[0040] The average particle size of the titanium nitride powder may be 20-100 nm, preferably 20-60 nm, such as 50 nm.
[0041] The mass percentage of the titanium nitride powder may be 10%-50%, preferably 20%-30%, for example 25%. The mass percentage indicates the mass percentage of the titanium nitride powder to the total mass of the titanium nitride powder, the silane coupling agent and the ethanol aqueous solution.
[0042] Wherein, the molecular formula of the silane coupling agent can be Y n SiX3, wherein n can be a natural number of 1-3, such as 1, 2 or 3. In the silane coupling agent, Y can include an acryloxy group, and preferably also includes one or more of a vinyl group, an allyl group, an alkyl group, a hydrogen group, an epoxy group and a mercapto group. The alkyl group can be a methyl group. X preferably includes one or more of a methoxy group, an ethoxy group, an acyloxy group, an aryloxy group and a tert-butyl peroxy group, such as a methoxy group.
[0043] The silane coupling agent is preferably KH-560, KH-570, A-174, KBM-503 or SH-6030, for example, KH-560 or KH-570.
[0044] The mass percentage of the silane coupling agent may be 10%-30%, preferably 12%-25%, such as 12.5%. The mass percentage indicates the mass percentage of the silane coupling agent to the total mass of the titanium nitride powder, the silane coupling agent and the ethanol aqueous solution.
[0045] The molar ratio of the titanium nitride powder to the silane coupling agent may be (5-10):1, preferably (6-9):1, such as 7.6:1 or 8:1.
[0046] The solvent A may be a conventional solvent in the art that can dissolve the titanium nitride powder and the silane coupling agent, such as an ethanol aqueous solution. In the ethanol aqueous solution, the mass ratio of ethanol to water may be (6-10):1, such as 9:1.
[0047] The reaction temperature may be 60-90°C, such as 70 or 80°C.
[0048] The reaction time may be 1-4 hours, such as 2 or 3 hours.
[0049] Wherein, the reaction can be carried out in a water bath or an oil bath.
[0050] After the reaction, washing and drying steps are generally included. The washing operation can be conventional in the art, such as centrifugal washing with ultrapure water. The drying operation can be conventional in the art, such as drying in an oven. The drying temperature can be 50-100°C, such as 70°C. The drying time can be 12-36h, such as 20h.
[0051] In the present invention, the average particle size of the modified titanium nitride powder is preferably 50-70 nm, preferably 50-58 nm.
[0052] In the present invention, the mass percentage of the dispersant is preferably 20%-55%, such as 25%, 30%, 40% or 50%; the above mass percentage represents the mass percentage of the dispersant to the total mass of the titanium nitride composite slurry.
[0053] In the present invention, the type of the dispersant may be a copolymer containing an acidic group. The acidic group may be a conventional group in the art that can generate hydrogen ions during hydrolysis or ionization, such as a carboxyl group and / or a sulfonic acid group. The dispersant is preferably a carboxylate copolymer, more preferably a styrene maleic anhydride copolymer, such as TEGO Dispers 670.
[0054] In the present invention, the mass percentage of the organic solvent B is preferably 30%-70%, such as 35%, 40%, 50% or 70%; the above mass percentage represents the mass percentage of the organic solvent B to the total mass of the titanium nitride composite slurry.
[0055] In the present invention, the non-polar solvent may be benzene and its derivatives, preferably xylene.
[0056] In the present invention, the fatty acid methyl ester may be a fatty acid methyl ester having 1 to 3 carbon atoms, preferably methyl acetate.
[0057] In the present invention, the organic solvent B is preferably xylene and / or methyl acetate.
[0058] In the present invention, the mixing method may be ball milling and / or sand milling, such as ball milling and sand milling.
[0059] The ball milling can be performed in a ball milling jar. The rotation speed during the ball milling can be 1000-2000 r / min, such as 1500 r / min. The ball milling time can be 10-50 min, such as 30 min.
[0060] The sand grinding can be performed in a sand mill. The rotation speed during the sand grinding can be 2000-4000 r / min, such as 2400 r / min. The sand grinding time can be 2-8 h, such as 6 h.
[0061] In a preferred embodiment, the mixing method is ball milling and sand milling, the rotation speed of the ball milling is 1000-2000 r / min, the time of the ball milling is 10-50 min, the rotation speed of the sand milling is 2000-4000 r / min, and the time of the sand milling is 2-8 h.
[0062] In a more preferred embodiment, the mixing method is ball milling and sand milling, the rotation speed during ball milling is 1500 r / min, the ball milling time is 30 min, the rotation speed during sand milling is 2400 r / min, and the sand milling time is 6 h.
[0063] In the sand grinding, zirconium beads are generally added, and the diameter of the zirconium beads can be 0.2 mm.
[0064] In a preferred embodiment, the method for preparing the titanium nitride composite slurry comprises the following steps:
[0065] (1) mixing and reacting titanium nitride powder, a silane coupling agent and a solvent A to obtain modified titanium nitride powder;
[0066] (2) mixing 10%-40% of modified titanium nitride powder, 15%-60% of a dispersant and 20%-75% of an organic solvent; the organic solvent is xylene and / or methyl acetate;
[0067] The mixing method is ball milling and sand milling; the rotation speed during the sand milling is 2000-4000r / min; the sand milling time is 2-8h; and the average particle size of the titanium nitride composite slurry is less than 100nm.
[0068] The present invention also provides a coating, which comprises the components other than the solvent in the titanium nitride composite slurry as described above and a resin.
[0069] In the present invention, the resin may be a conventional resin in the art, such as an epoxy resin and / or an acrylic resin.
[0070] In the present invention, the mass ratio of the titanium nitride composite slurry to the resin may be 1:(3-8), for example, 1:5.
[0071] In the present invention, the raw material of the coating preferably further comprises a solvent. The solvent may be xylene and / or methyl acetate. The mass ratio of the titanium nitride composite slurry to the solvent may be 1:(3-8), for example 1:5.
[0072] The present invention also provides a method for preparing the coating as described above, which comprises mixing the titanium nitride composite slurry and resin as described above and removing the solvent.
[0073] In the present invention, the method for removing the solvent can be conventional in the art, such as drying. The drying temperature can be 90-110° C., such as 110° C. The drying time can be 1-3 min, such as 2 min.
[0074] The present invention also provides an application of the titanium nitride composite slurry or coating as described above in the field of thermal insulation materials.
[0075] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0076] The reagents and raw materials used in the present invention are commercially available.
[0077] The positive and progressive effects of the present invention are:
[0078] The titanium nitride composite slurry prepared by the present invention is evenly dispersed, the system is stable, and a high-efficiency infrared blocking effect can be achieved. The preparation process of the present invention is simple and easy to operate, and batch industrial production can be carried out, and it can be directly used in the fields of vehicle films, building glass window films, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0079] Figure 1 This is the microscopic morphology of the modified titanium nitride powder prepared in Example 1. DETAILED DESCRIPTION
[0080] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0081] Example 1
[0082] (1) Preparation of modified titanium nitride powder: 20 parts of titanium nitride powder (average particle size of 60 nm) and 10 parts of silane coupling agent KH-570 and 50 parts of ethanol aqueous solution were mixed evenly, wherein the mass ratio of ethanol to water was 9:1. The mixed solution was placed in an 80°C oil bath and heated under reflux for 2 h to allow the powder surface to fully contact the coupling agent. After the reaction was completed, it was washed several times by centrifugation with ultrapure water and then placed in an oven at 70°C overnight. The molar ratio of titanium nitride powder to silane coupling agent was 8:1.
[0083] (2) 20 parts of modified titanium nitride powder, 30 parts of dispersant styrene maleic anhydride copolymer (TEGO Dispers 670), and 50 parts of xylene organic solvent were placed in a ball mill, pre-mixed at 1500 r / min for 30 minutes, and then transferred to a sand mill and sand-milled at 2400 r / min for 6 hours using 0.2 mm zirconium beads to obtain a titanium nitride composite slurry.
[0084] Example 2
[0085] The organic solvent xylene in Example 1 was replaced with methyl acetate, and the other experimental conditions were the same as those in Example 1.
[0086] Example 3
[0087] The raw material ratio in step (2) of Example 1 was replaced with 20 parts of modified titanium nitride powder, 40 parts of dispersant, and 40 parts of xylene organic solvent. The other experimental conditions were the same as those in Example 1.
[0088] Example 4
[0089] The silane coupling agent in step (1) of Example 1 was replaced with KH-560 (γ-(2,3-epoxypropoxy)propyltrimethoxysilane), and the other experimental conditions were the same as those of Example 1. The molar ratio of titanium nitride powder to the silane coupling agent was 7.6:1.
[0090] Example 5
[0091] The amount of modified titanium nitride powder in Example 1 was changed to 35 parts, the amount of organic solvent was changed to 35 parts, and the other experimental conditions were the same as those in Example 1.
[0092] Example 6
[0093] The dispersant in Example 1 was changed to 50 parts of styrene maleic anhydride copolymer (TEGO Dispers670), the organic solvent was changed to 30 parts, and the other experimental conditions were the same as those in Example 1.
[0094] Comparative Example 1
[0095] The organic solvent xylene in Example 1 was replaced with methyl benzoate, and the other experimental conditions were the same as those in Example 1.
[0096] Comparative Example 2
[0097] The sanding time in step (2) of Example 1 was extended to 9 h, and the other experimental conditions were the same as those in Example 1.
[0098] Comparative Example 3
[0099] Except that the dispersant in Example 1 was changed to polyurethane dispersant EFKA4063, other experimental conditions were the same as those in Example 1.
[0100] Comparative Example 4
[0101] The dispersant styrene maleic anhydride copolymer (TEGO Dispers 670) in Example 1 was changed to 10 parts, the organic solvent was changed to 70 parts, and the other experimental conditions were the same as in Example 1.
[0102] Effect Example 1
[0103] The modified titanium nitride powder obtained in Example 1 was observed by SEM, and the results were as follows: Figure 1 .Depend on Figure 1 It can be seen that the modified titanium nitride powder prepared in Example 1 has no obvious agglomeration phenomenon, is evenly dispersed, and has a small particle size (50 nm).
[0104] Effect Example 2
[0105] The average particle size of the modified titanium nitride powders prepared in the examples and comparative examples was tested by SEM testing, where a single particle was measured by high-magnification SEM (10000X), 3 different points were randomly selected, 5 particles were measured at each point, and the average value was taken.
[0106] The average particle size of the titanium nitride composite slurry prepared in the embodiment and the comparative example was tested. A nanoparticle size tester was used to test, and 5 μL of the titanium nitride composite slurry prepared in the above embodiment and the comparative example was respectively taken with a pipette gun, and the above titanium nitride composite slurry was diluted to 50 mL with a solvent of the same type as the organic solvent B in the preparation example, and 1.5 mL of the diluted titanium nitride composite slurry was taken into a glass dish, placed in the nanoparticle size tester to test the particle size, and the data was read.
[0107] The titanium nitride composite slurry prepared in the embodiment and the comparative example was subjected to a coating test. The coating solution was prepared in the following ratio: 1 g slurry + 5 g solvent (xylene) + 5 g resin (acrylic resin, model: Ashland 951059). The prepared coating solution was coated on a Toray transparent PET film using a coater, and heated in an oven at 100°C for 2 min for configuration. The infrared blocking condition (940 nm infrared blocking rate, 1400 nm infrared blocking rate, and total infrared blocking rate) and visible light transmittance of the coating prepared by the titanium nitride composite slurry were tested using a solar film tester, and the haze of the coating prepared by the titanium nitride composite slurry was tested using a desktop colorimeter.
[0108] The 940nm infrared rejection rate is the infrared rejection rate obtained at a wavelength of 940nm.
[0109] The total infrared rejection rate is the infrared rejection rate obtained at a wavelength of 780nm-1mm.
[0110] The 1400nm infrared rejection rate is the infrared rejection rate obtained at a wavelength of 1400nm.
[0111] Visible light transmittance refers to the degree of visible light transmission in the visible light band (wavelength range is approximately 380nm to 780nm).
[0112] The haze is tested using a desktop colorimeter. By adjusting the desktop colorimeter in transmission mode, the above coating is placed at the test point, and the moving coating is tested in three different places to take the average value.
[0113] The coating test results are shown in Table 1:
[0114] Table 1
[0115]
[0116]
[0117] Compared with the comparative example, the coatings prepared by the titanium nitride composite slurry obtained by using specific organic solvents in Examples 1-6 at a specific mass percentage have better infrared blocking effects (940nm infrared blocking rate, 1400nm infrared blocking rate and full infrared blocking rate are better) and visible light transmittance.
Claims
1. A titanium nitride composite slurry, characterized in that: It includes the following components in percentage by mass: 10%-40% modified titanium nitride powder; 15%-60% dispersant; 20%-75% organic solvent B; the organic solvent B is a non-polar solvent and / or fatty acid methyl ester; the average particle size of the titanium nitride composite slurry is less than 100nm; The modified titanium nitride powder is titanium nitride powder modified by a silane coupling agent; The above mass percentages represent the percentage of the mass of each component to the total mass of the titanium nitride composite slurry.
2. The titanium nitride composite slurry according to claim 1, characterized in that: The titanium nitride composite slurry meets one or more of the following conditions: (1) The mass percentage of the modified titanium nitride powder is 18%-38%, for example, 20% or 35%; (2) The mass percentage of the dispersant is 20%-55%, for example, 25%, 30%, 40% or 50%; (3) the mass percentage of the organic solvent B is 30%-70%, for example 35%, 40%, 50% or 70%; and, (4) The average particle size of the titanium nitride composite slurry is less than 98 nm, for example, 94, 92, 84, 77, 48, 50, 51, 52 nm or 69 nm.
3. The titanium nitride composite slurry according to claim 2, characterized in that: The titanium nitride composite slurry meets one or more of the following conditions: (1) The average particle size of the modified titanium nitride powder is 50-70 nm, preferably 50-58 nm; (2) The method for preparing the modified titanium nitride powder comprises mixing a silane coupling agent and titanium nitride powder, preferably comprising mixing and reacting titanium nitride powder, a silane coupling agent and a solvent A; (3) The dispersant is a copolymer containing an acidic group; the acidic group is preferably a carboxyl group and / or a sulfonic acid group; (4) The non-polar solvent is benzene and its derivatives, preferably xylene; (5) the fatty acid methyl ester is a fatty acid methyl ester having 1 to 3 carbon atoms, preferably methyl acetate; and, (6) The organic solvent B is xylene and / or methyl acetate.
4. The titanium nitride composite slurry according to claim 3, characterized in that: The titanium nitride composite slurry meets one or more of the following conditions: (1) The average particle size of the titanium nitride powder is 20-100 nm, preferably 20-60 nm, for example 50 nm; (2) The mass percentage of the titanium nitride powder is 10%-50%, preferably 20%-30%, for example 25%; the mass percentage indicates the mass percentage of the titanium nitride powder to the total mass of the titanium nitride powder, the silane coupling agent and the ethanol aqueous solution; (3) The molecular formula of the silane coupling agent is Y n SiX3, wherein n is a natural number of 1-3, such as 1, 2 or 3; in the silane coupling agent, the Y preferably includes an acryloxy group, and preferably also includes one or more of a vinyl group, an allyl group, an alkyl group, a hydrogen group, an epoxy group and a mercapto group; the alkyl group is preferably a methyl group; the X preferably includes one or more of a methoxy group, an ethoxy group, an acyloxy group, an aryloxy group and a tert-butyl peroxy group, such as a methoxy group; the silane coupling agent is preferably KH-560, KH-570, A-174, KBM-503 or SH-6030, such as KH-560 or KH-570; (4) The mass percentage of the silane coupling agent is 10%-30%, preferably 12%-25%, for example 12.5%; the mass percentage indicates the mass percentage of the silane coupling agent to the total mass of the titanium nitride powder, the silane coupling agent and the ethanol aqueous solution; (5) the molar ratio of the titanium nitride powder to the silane coupling agent is (5-10):1, preferably (6-9):1, for example 7.6:1 or 8:1; and, (6) The solvent A is an ethanol aqueous solution; the mass percentage of the solvent A is preferably 40%-70%, more preferably 50%-65%, for example 62.5%; the mass percentage represents the mass of the solvent A as a percentage of the total mass of the titanium nitride powder, the silane coupling agent and the solvent A.
5. A method for preparing a titanium nitride composite slurry, characterized in that: It includes the following steps: 10%-40% of modified titanium nitride powder, 15%-60% of dispersant and 20%-75% of organic solvent B are mixed; the organic solvent B is a non-polar solvent and / or fatty acid methyl ester; the average particle size of the titanium nitride composite slurry is less than 100nm; the above mass percentage represents the percentage of the mass of each component to the total mass of the titanium nitride composite slurry; The modified titanium nitride powder is titanium nitride powder modified by a silane coupling agent.
6. The method for preparing the titanium nitride composite slurry according to claim 5, characterized in that: The method for preparing the titanium nitride composite slurry satisfies one or more of the following conditions: (1) The mass percentage of the modified titanium nitride powder is 18%-38%, for example, 20% or 35%; (2) The average particle size of the modified titanium nitride powder is 50-70 nm, preferably 50-58 nm; (3) The method for preparing the modified titanium nitride powder comprises mixing a silane coupling agent and titanium nitride powder, preferably comprising mixing and reacting titanium nitride powder, a silane coupling agent and a solvent A; Wherein, the average particle size of the titanium nitride powder is preferably 20-100 nm, more preferably 20-60 nm, for example 50 nm; Wherein, the mass percentage of the titanium nitride powder is preferably 10%-50%, more preferably 20%-30%, for example 25%; the mass percentage represents the mass percentage of the titanium nitride powder to the total mass of the titanium nitride powder, the silane coupling agent and the ethanol aqueous solution; Wherein, the molecular formula of the silane coupling agent is Y n SiX3, wherein n is preferably a natural number of 1-3, such as 1, 2 or 3; in the silane coupling agent, Y preferably includes an acryloxy group, and preferably also includes one or more of a vinyl group, an allyl group, an alkyl group, a hydrogen group, an epoxy group and a mercapto group; the alkyl group is preferably a methyl group; X preferably includes one or more of a methoxy group, an ethoxy group, an acyloxy group, an aryloxy group and a tert-butyl peroxy group, such as a methoxy group; the silane coupling agent is preferably KH-560, KH-570, A-174, KBM-503 or SH-6030, such as KH-560 or KH-570; Wherein, the mass percentage of the silane coupling agent is preferably 10%-30%, preferably 12%-25%, for example 12.5%; the mass percentage indicates the mass percentage of the silane coupling agent to the total mass of the titanium nitride powder, the silane coupling agent and the ethanol aqueous solution; Wherein, the molar ratio of the titanium nitride powder to the silane coupling agent is preferably (5-10):1, preferably (6-9):1, for example 7.6:1 or 8:1; Wherein, the solvent A is preferably an ethanol aqueous solution; the mass percentage of the solvent A is preferably 40%-70%, more preferably 50%-65%, for example 62.5%; the mass percentage represents the mass percentage of the solvent A to the total mass of the titanium nitride powder, the silane coupling agent and the solvent A. (4) The mass percentage of the dispersant is 20%-55%, for example, 25%, 30%, 40% or 50%; (5) The dispersant is a copolymer containing an acidic group; the acidic group is preferably a carboxyl group and / or a sulfonic acid group; (6) The non-polar solvent is benzene and its derivatives, preferably xylene; (7) The fatty acid methyl ester is a fatty acid methyl ester having 1 to 3 carbon atoms, preferably methyl acetate; (8) The mass percentage of the organic solvent B is 30%-70%, for example 35%, 40%, 50% or 70%; (9) the organic solvent B is xylene and / or methyl acetate; and, (10) The average particle size of the titanium nitride composite slurry is less than 98 nm, for example, 94, 92, 84, 77, 48, 50, 51, 52 nm or 69 nm.
7. The method for preparing the titanium nitride composite slurry according to claim 5, characterized in that: The mixing method is ball milling and / or sand milling, such as ball milling and sand milling; The rotation speed during the ball milling is preferably 1000-2000 r / min, such as 1500 r / min; the time of the ball milling is preferably 10-50 min, such as 30 min; The rotation speed during the sand grinding is preferably 2000-4000 r / min, such as 2400 r / min; and the time of the sand grinding is preferably 2-8 h, such as 6 h.
8. A coating, characterized in that It comprises the components other than the solvent in the titanium nitride composite slurry according to any one of claims 1 to 4 and a resin; The resin is preferably an epoxy resin and / or an acrylic resin; The mass ratio of the titanium nitride composite slurry to the resin is preferably 1:(3-8), for example 1:
5.
9. A method for preparing a coating as claimed in claim 8, characterized in that: The titanium nitride composite slurry according to any one of claims 1 to 4 is mixed with a resin and the solvent is removed.
10. Use of the titanium nitride composite slurry according to any one of claims 1 to 4, or the coating according to claim 8 in the field of thermal insulation materials.
Citation Information
Patent Citations
Aqueous self-cleaning transparent heat-insulated nano-dope capable of fully shielding infrared ray and ultraviolet ray
CN102732108A
Full-shielded infrared and ultraviolet polyurethane nanometer transparent heat insulating coating
CN102746781A
Cesium tungsten bronze slurry and preparation method and application thereof
CN116120775A
Optical recording medium containing IR-ray absorptive compound