High-elastic crease-resistant linen antibacterial fabric and preparation method thereof
By modifying flax fiber and blending it with other fibers, combined with the use of antibacterial finishing liquid, the problems of the hardness and insufficient antibacterial properties of flax fabrics are solved, the preparation of highly elastic and antibacterial fabrics is achieved, and the use of the fabrics is extended. life.
Patent Information
- Application Number
- CN202410797433.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-20
AI Technical Summary
Due to its hardness and lack of elasticity, linen fabric is prone to wrinkles and deformation, leading to fabric damage, and does not have antibacterial properties.
By blending flax fiber with polyester fiber and polyacrylonitrile fiber, and modifying the flax fiber, including using mandelic acid and terephthalic acid for esterification, it improves its softness and bonding properties, and adopts antibacterial finishing. Liquid treats fabrics to enhance antimicrobial properties.
It improves the tensile properties and softness of linen fiber, giving the blended fabric good elasticity and antibacterial properties, preventing wrinkles and bacterial growth, and extending the service life of the fabric.
Smart Images

Figure BDA0004902203370000071 
Figure BDA0004902203370000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of linen fabrics, and in particular to a high-elastic wrinkle-resistant antibacterial linen fabric and a preparation method thereof. Background Art
[0002] Flax is the earliest natural plant fiber used by humans, with a history of more than 10,000 years. As flax has excellent moisture absorption and moisture conductivity, and can absorb more than 20 times its own weight in water, linen fabrics are breathable, cool, crisp and comfortable, and are very popular among consumers, with a very broad market.
[0003] Although linen fabric has many advantages, it is a plant fiber with a hard feel and basically has no elasticity. It is prone to wrinkles during use, and it is easy to deform due to stretching, resulting in fabric damage. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a high-elastic wrinkle-resistant linen antibacterial fabric and a preparation method thereof.
[0005] The technical solution of the present invention is: a highly elastic and wrinkle-resistant linen antibacterial fabric, characterized in that it is made by blending 50 to 60 parts of linen fibers, 20 to 30 parts of polyester fibers, and 10 to 20 parts of polyacrylonitrile fibers; the linen fibers are modified before blending to obtain modified linen fibers.
[0006] Description: The flax fiber of the above antibacterial fabric has been modified to improve the tensile properties of the flax fiber and make the flax fiber softer. The modified flax fiber can be well combined with polyester fiber and polyacrylonitrile fiber, so that the blended fabric has good elasticity and can effectively prevent wrinkles.
[0007] Furthermore, the modification method is:
[0008] S1. Add mandelic acid into an ethanol solution 2 to 3 times its own weight, and stir for 10 to 15 minutes to obtain a mixed solution;
[0009] S2. Immerse the flax fiber in the mixed solution, wherein the mass ratio of the flax fiber to the mixed solution is 1:3-5, and keep the mixed solution at 60-70° C. for 1-2 hours. During the keeping process, add terephthalic acid to the mixed solution every 30-40 minutes, and the single addition amount of terephthalic acid accounts for 4-6% of the total mass of the flax fiber.
[0010] S3. After the first heat preservation is completed, add 2-4% of boric acid to the mixed solution, and then place the mixed solution at 100-120° C. for a second heat preservation time of 2-3 hours. After the second heat preservation is completed, wash and dry the flax fiber to obtain modified flax fiber.
[0011] Description: The above modification treatment improves the tensile properties of flax fiber and makes it softer through the esterification reaction between mandelic acid and the hydroxyl groups on flax fiber. In addition, terephthalic acid can react with the hydroxyl groups on flax fiber to improve the bonding between flax fiber and polyester fiber, ensuring that the blended fabric has good tensile properties.
[0012] Furthermore, the mass concentration of the ethanol solution is 50-75%.
[0013] Note: The above concentration of ethanol solution can ensure that mandelic acid fully penetrates into the flax fiber to ensure the effect of the modification treatment.
[0014] Furthermore, the cleaning method comprises soaking the flax fibers in a flowing detergent, the detergent temperature is 30-40° C., the soaking time is 20-25 minutes, and after the soaking is completed, the flax fibers are rinsed with clean water for 3-5 times.
[0015] Note: The above cleaning method can effectively remove impurities attached to the surface of flax fibers to avoid affecting the subsequent blending effect.
[0016] Furthermore, during the secondary heat preservation, the mixed solution is placed in a pressure vessel, and nitrogen is filled into the pressure vessel to make the pressure in the pressure vessel reach 0.6-0.8 MPa.
[0017] Note: Filling with nitrogen can increase the pressure of the reaction system, increase the collision frequency and energy between reactant molecules, promote the esterification reaction, and accelerate the reaction rate.
[0018] On the other hand, the present invention provides a method for preparing a highly elastic and wrinkle-resistant linen antibacterial fabric, which is used to prepare the antibacterial fabric, comprising the following steps:
[0019] Step 1, feeding the modified flax fiber, polyester fiber and polyacrylonitrile fiber into a blending machine according to a proportion, and blending them in the blending machine to obtain mixed spinning;
[0020] Step 2: Weaving the mixed yarn to obtain linen fabric, and then performing antibacterial finishing on the linen fabric to obtain antibacterial fabric.
[0021] Description: The linen fabric prepared by the above preparation method has good elasticity, and the antibacterial finishing improves the antibacterial performance of the linen fabric, making it difficult for bacteria to grow on the surface of the linen fabric, thereby improving the durability and durability of the fabric.
[0022] Furthermore, the antibacterial finishing method is: heating the antibacterial finishing liquid to 30-40°C, then immersing the linen fabric in the antibacterial finishing liquid, taking out the linen fabric every 3-5 minutes during the immersion process for air drying, the single air drying time is 15-20 minutes, the wind speed is 10-12 m / s, until the antibacterial fabric is obtained after air drying 2-4 times, and the temperature of the antibacterial finishing liquid is increased by 5-8°C after each air drying.
[0023] Note: The above antibacterial finishing method first uses an antibacterial finishing liquid to soak the linen fabric, and then air-dries it multiple times to form an antibacterial layer on the linen fabric to reduce bacterial growth and reduce the generation of odor during the use of the fabric.
[0024] Furthermore, the ingredients of the antibacterial finishing liquid include, by weight: 15-25 parts of sodium dodecyl sulfate, 5-10 parts of disodium hydrogen phosphate, 3-8 parts of silver nitrate, 5-10 parts of sodium salicylate, 2-4 parts of polydimethylsiloxane, and 50-75 parts of deionized water.
[0025] Description: After finishing linen fabrics with the above antibacterial finishing liquid, the growth of microorganisms such as bacteria and fungi on the surface of the textile fabrics can be inhibited, the growth and reproduction of bacteria on the fabrics can be reduced, and the fabrics can be kept clean and hygienic.
[0026] The beneficial effects of the present invention are:
[0027] (1) The flax fiber of the antibacterial fabric of the present invention has been modified to improve the tensile properties of the flax fiber and make the flax fiber softer. The modified flax fiber can be well combined with polyester fiber and polyacrylonitrile fiber, so that the blended fabric has good elasticity and can effectively prevent wrinkles.
[0028] (2) The modification treatment of the present invention improves the tensile properties of the flax fiber by an esterification reaction between mandelic acid and the hydroxyl groups on the flax fiber, making the flax fiber softer. In addition, terephthalic acid can react with the hydroxyl groups on the flax fiber to improve the bonding between the flax fiber and the polyester fiber, thereby ensuring that the blended fabric has good tensile properties.
[0029] (3) The linen fabric prepared by the preparation method of the present invention has good elasticity, and the linen fabric after antibacterial finishing can effectively inhibit the growth of microorganisms such as bacteria and fungi, reduce the generation of odor during the use of the fabric, and improve the durability and durability of the fabric. DETAILED DESCRIPTION
[0030] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.
[0031] Example 1: A highly elastic and wrinkle-resistant linen antibacterial fabric, which is blended from 55 parts of linen fiber, 25 parts of polyester fiber, and 15 parts of polyacrylonitrile fiber; the linen fiber is modified before blending to obtain modified linen fiber;
[0032] The modification method is:
[0033] S1. Add mandelic acid into an ethanol solution of 2.5 times its own weight, stir for 12 minutes, and obtain a mixed solution; the mass concentration of the ethanol solution is 60%;
[0034] S2. Immerse the flax fiber in the mixed solution, the mass ratio of the flax fiber to the mixed solution is 1:4, and keep the mixed solution at 65°C for 1.5 hours. During the insulation process, add terephthalic acid to the mixed solution every 35 minutes, and the single addition amount of terephthalic acid accounts for 5% of the total mass of the flax fiber;
[0035] S3. After the first insulation is completed, 3% of the total mass of boric acid is added to the mixed solution, and then the mixed solution is placed at 110° C. for a second insulation, the second insulation time is 2.5 hours, and during the second insulation, the mixed solution is placed in a pressure vessel, and nitrogen is filled into the pressure vessel to make the pressure in the pressure vessel reach 0.7 MPa. After the second insulation is completed, the flax fiber is washed and dried to obtain modified flax fiber; the washing method is to soak the flax fiber in a flowing detergent, the detergent temperature is 35° C., the soaking time is 22 minutes, and after the soaking is completed, it is rinsed with clean water for 4 times, the detergent components include 30% stearic acid, 8% sodium carbonate, 15% alkylphenol polyoxyethylene ether by mass percentage, and the balance is water, and the flow rate of the detergent is 0.5 m / s.
[0036] The preparation method of the above-mentioned high-elastic wrinkle-resistant linen antibacterial fabric comprises the following steps:
[0037] Step 1, feeding the modified flax fiber, polyester fiber and polyacrylonitrile fiber into a blending machine according to a proportion, and blending them in the blending machine to obtain mixed spinning;
[0038] Step 2, weaving the mixed yarn to obtain linen fabric, and then performing antibacterial finishing on the linen fabric to obtain antibacterial fabric;
[0039] The antibacterial finishing method is as follows: the antibacterial finishing liquid is heated to 35°C, and then the linen fabric is immersed in the antibacterial finishing liquid. During the immersion process, the linen fabric is taken out once every 4 minutes for air drying. The single air drying time is 18 minutes, and the wind speed is 11m / s, until the antibacterial fabric is obtained after air drying 3 times, and the temperature of the antibacterial finishing liquid is increased by 7°C after each air drying. The ingredients of the antibacterial finishing liquid include, by weight: 20 parts of sodium dodecyl sulfate, 8 parts of disodium hydrogen phosphate, 5 parts of silver nitrate, 8 parts of sodium salicylate, 3 parts of polydimethylsiloxane, and 60 parts of deionized water.
[0040] Example 2: This example is basically the same as Example 1, except that the antibacterial fabric is made by blending 50 parts of flax fiber, 20 parts of polyester fiber, and 10 parts of polyacrylonitrile fiber.
[0041] Example 3: This example is basically the same as Example 1, except that the antibacterial fabric is made by blending 60 parts of flax fiber, 30 parts of polyester fiber, and 20 parts of polyacrylonitrile fiber.
[0042] Example 4: This example is basically the same as Example 1, except that the flax fibers are immersed in the mixed solution, and the mixed solution is kept warm at 60° C. for 1 hour.
[0043] Example 5: This example is basically the same as Example 1, except that the flax fibers are immersed in the mixed solution, and the mixed solution is kept warm at 70° C. for 2 hours.
[0044] Example 6: This example is basically the same as Example 1, except that the single addition amount of terephthalic acid accounts for 4% of the total mass of the flax fiber.
[0045] Example 7: This example is basically the same as Example 1, except that the single addition amount of terephthalic acid accounts for 6% of the total mass of the flax fiber.
[0046] Example 8: This example is basically the same as Example 1, except that the mixed solution is placed at 100°C for secondary insulation, and the secondary insulation time is 2 hours.
[0047] Example 9: This example is basically the same as Example 1, except that the mixed solution is placed at 120°C for secondary insulation, and the secondary insulation time is 3 hours.
[0048] Example 10: This example is basically the same as Example 1, except that the antibacterial fabric is obtained after air-drying twice.
[0049] Example 11: This example is basically the same as Example 1, except that the antibacterial fabric is obtained after air-drying 4 times.
[0050] Example 12: This example is basically the same as Example 1, except that the temperature of the antibacterial finishing liquid is increased by 5°C after each air-drying.
[0051] Example 13: This example is basically the same as Example 1, except that the temperature of the antibacterial finishing liquid is increased by 8°C after each air-drying.
[0052] Example 14: This example is basically the same as Example 1, except that the ingredients of the antibacterial finishing liquid include, by weight: 15 parts of sodium lauryl sulfate, 5 parts of disodium hydrogen phosphate, 3 parts of silver nitrate, 5 parts of sodium salicylate, 2 parts of polydimethylsiloxane, and 50 parts of deionized water.
[0053] Example 15: This example is basically the same as Example 1, except that the ingredients of the antibacterial finishing liquid include, by weight: 25 parts of sodium lauryl sulfate, 10 parts of disodium hydrogen phosphate, 8 parts of silver nitrate, 10 parts of sodium salicylate, 4 parts of polydimethylsiloxane, and 75 parts of deionized water.
[0054] Experimental example: In order to explore the influence of the parameters of each embodiment on the performance of the fabric, the method described in FZ-T70006-2022 was used to test the fabric of each embodiment to obtain the tensile elastic recovery rate of the sample of each embodiment; the bacterial liquid absorption method was used to test the antibacterial rate of the fabric of each embodiment against Escherichia coli, and the specific exploration is as follows:
[0055] 1. Explore the influence of fabric composition on fabric performance
[0056] Examples 1, 2, and 3 were used as experimental comparisons, and Example 1 was used as a reference. The flax fiber was not subjected to modification treatment as Comparative Example 1. The fabric properties under different fabric compositions were shown in Table 1 below:
[0057] Table 1 Fabric properties under different fabric compositions
[0058] Group Tensile elastic recovery rate (%) Escherichia coli inhibition rate (%) Example 1 81.36 89.23 Example 2 79.25 88.65 Example 3 78.69 87.96 Comparative Example 1 68.52 87.48
[0059] It can be seen from the data in Table 1 that compared with Examples 1, 2, and 3, the fabric in Example 1 has the best tensile elastic recovery rate, indicating that the elastic performance of the fabric obtained by the components of Example 1 is the best, while the antibacterial performance is not much different, indicating that the fabric composition has little effect on the antibacterial performance of the fabric; compared with Comparative Example 1, the tensile elastic recovery rate of the fabric in Comparative Example 1 is significantly reduced, indicating that the elasticity of the fabric can be improved after the flax fiber is modified.
[0060] 2. Explore the influence of primary insulation parameters on fabric performance
[0061] Examples 1, 4, and 5 were used as experimental comparisons, and Example 1 was used as a reference, with a primary insulation temperature of 80° C. and a thermal insulation time of 1.5 h as comparative example 2. The fabric performance under different primary insulation parameters is shown in Table 2 below:
[0062] Table 2 Fabric performance under different parameters of primary insulation
[0063] Group Tensile elastic recovery rate (%) Escherichia coli inhibition rate (%) Example 1 81.36 89.23 Example 4 80.95 88.35 Example 5 79.94 88.54 Comparative Example 2 72.66 87.97
[0064] It can be seen from the data in Table 2 that compared with Examples 1, 4 and 5, the fabric tensile elastic recovery rate of Example 1 is the best. This may be because under the primary insulation parameters of Example 1, mandelic acid and flax fiber can fully react, so the primary insulation parameters selected in Example 1 are optimal. Compared with Comparative Example 2, the fabric tensile elastic recovery rate of Comparative Example 2 decreases in Example 1. This may be because the insulation temperature is too high, resulting in a large amount of ethanol evaporation.
[0065] 3. Explore the effect of terephthalic acid addition on fabric performance
[0066] Examples 1, 6, and 7 were used as experimental comparisons. Example 1 was used as a reference. The terephthalic acid was added all at once as comparative example 3. The fabric properties obtained under different addition amounts of terephthalic acid were shown in Table 3 below:
[0067] Table 3 Fabric properties at different addition amounts of terephthalic acid
[0068] Group Tensile elastic recovery rate (%) Escherichia coli inhibition rate (%) Example 1 81.36 89.23 Example 6 80.25 88.37 Example 7 81.45 89.29 Comparative Example 3 77.68 87.66
[0069] It can be seen from the data in Table 3 that compared with Examples 1 and 6, the tensile elastic recovery rate of the fabric in Example 1 is better, which may be because the terephthalic acid reacts fully. Compared with Example 7, there is little difference between Example 1 and Example 7. Therefore, from a cost perspective, the amount of terephthalic acid added selected in Example 1 is optimal; compared with Comparative Example 3, the tensile elastic recovery rate of the fabric in Comparative Example 3 decreases, which may be because terephthalic acid cannot be evenly dispersed in the mixed solution after being added once.
[0070] 4. Explore the influence of secondary insulation parameters on fabric performance
[0071] Examples 1, 8, and 9 were used as experimental comparisons, and Example 1 was used as a reference. The secondary insulation temperature was 140° C. and the time was 2.5 h as Comparative Example 4. The fabric performance under different secondary insulation parameters was shown in Table 4 below:
[0072] Table 4 Fabric performance under different parameters of secondary insulation
[0073] Group Tensile elastic recovery rate (%) Escherichia coli inhibition rate (%) Example 1 81.36 89.23 Example 8 80.51 88.78 Example 9 80.35 89.02 Comparative Example 4 78.26 88.79
[0074] It can be seen from the data in Table 2 that compared with Examples 1, 8 and 9, the fabric tensile elastic recovery rate of Example 1 is the best. This may be because under the secondary insulation parameters of Example 1, terephthalic acid can fully react, so the secondary insulation parameters selected in Example 1 are optimal. Compared with Comparative Example 4, the fabric tensile elastic recovery rate of Comparative Example 4 decreases. This may be because the temperature is too high, resulting in the inability of terephthalic acid to fully react.
[0075] 5. Explore the impact of air drying times on fabric performance
[0076] Examples 1, 10, and 11 were used as experimental comparisons. Example 1 was used as a reference, and the air-drying step was performed only once as comparative example 5. The fabric properties obtained under different air-drying times are shown in Table 5 below:
[0077] Table 5 Fabric properties under different air drying times
[0078] Group Tensile elastic recovery rate (%) Escherichia coli inhibition rate (%) Example 1 81.36 89.23 Example 10 81.44 87.29 Embodiment 11 81.28 89.26 Comparative Example 5 81.35 85.62
[0079] It can be seen from the data in Table 3 that compared with Comparative Example 5, as the number of air-drying times increases, the tensile elastic recovery rate of the fabric in Examples 1, 10, and 11 does not change significantly, which indicates that the antibacterial finishing has little effect on the tensile elastic recovery rate of the fabric, and the Escherichia coli antibacterial rate of the fabric gradually increases until it reaches the highest in Example 1. However, as the number of air-drying times continues to increase, the Escherichia coli antibacterial rate does not change significantly, so the number of air-drying times selected in Example 1 is optimal.
[0080] 6. Explore the effect of temperature change of antibacterial finishing liquid on fabric performance
[0081] Examples 1, 12, and 13 were used as experimental comparisons, and Example 1 was used as a reference, and the temperature of the antibacterial finishing liquid was unchanged as comparative example 6. The fabric properties under different temperature changes of the antibacterial finishing liquid were shown in Table 6 below:
[0082] Table 6 Fabric properties under different temperature changes of antibacterial finishing liquid
[0083]
[0084]
[0085] It can be seen from the data in Table 6 that compared with Examples 1, 12 and 13, Example 1 has the highest antibacterial rate of Escherichia coli. This may be because gradually increasing the temperature of the antibacterial finishing liquid helps the antibacterial finishing liquid to penetrate into the pores of the fabric and improve the antibacterial finishing effect. Therefore, the temperature change of the antibacterial finishing liquid selected in Example 1 is optimal. Compared with Comparative Example 6, the antibacterial effect of the fabric of Comparative Example 6 decreased in Example 1. This may be because the antibacterial finishing liquid cannot fully penetrate into the fabric, resulting in the antibacterial finishing effect being affected.
[0086] 7. Explore the influence of the composition of antibacterial finishing liquid on fabric performance
[0087] Using Examples 1, 14, and 15 as experimental comparative examples, and Example 1 as a reference, a commercially available antibacterial finishing liquid was used as comparative example 7, and the fabric properties under different components of the antibacterial finishing liquid were obtained as shown in Table 7 below:
[0088] Table 7 Fabric properties under different temperature changes of antibacterial finishing liquid
[0089] Group Tensile elastic recovery rate (%) Escherichia coli inhibition rate (%) Example 1 81.36 89.23 Embodiment 14 81.35 88.14 Embodiment 15 81.29 88.26 Comparative Example 7 81.14 84.34
[0090] It can be seen from the data in Table 7 that compared with Examples 1, 14 and 15, Example 1 has the highest antibacterial rate of Escherichia coli. This may be because the antibacterial finishing liquid components of Example 1 are more uniform and have better antibacterial effects. Therefore, the antibacterial finishing liquid components selected in Example 1 are better. Compared with Comparative Example 7, the antibacterial effect of the fabric of Comparative Example 7 decreased in Example 1, which indicates that the antibacterial finishing liquid of the present application has better effects.
Claims
1. A highly elastic and wrinkle-resistant linen antibacterial fabric, characterized in that: The modified flax fiber is prepared by blending 50-60 parts of flax fiber, 20-30 parts of polyester fiber and 10-20 parts of polyacrylonitrile fiber; the flax fiber is modified before blending to obtain modified flax fiber.
2. The high-elastic wrinkle-resistant linen antibacterial fabric according to claim 1, characterized in that: The modification method is: S1. Add mandelic acid into an ethanol solution 2 to 3 times its own weight, and stir for 10 to 15 minutes to obtain a mixed solution; S2. Immerse the flax fiber in the mixed solution, wherein the mass ratio of the flax fiber to the mixed solution is 1:3-5, and keep the mixed solution at 60-70° C. for 1-2 hours. During the keeping process, add terephthalic acid to the mixed solution every 30-40 minutes, and the single addition amount of terephthalic acid accounts for 4-6% of the total mass of the flax fiber. S3. After the first heat preservation is completed, add 2-4% of boric acid to the mixed solution, and then place the mixed solution at 100-120° C. for a second heat preservation time of 2-3 hours. After the second heat preservation is completed, wash and dry the flax fiber to obtain modified flax fiber.
3. The high-elastic wrinkle-resistant linen antibacterial fabric according to claim 2, characterized in that: The mass concentration of the ethanol solution is 50-75%.
4. The high-elastic wrinkle-resistant linen antibacterial fabric according to claim 2, characterized in that: The cleaning method comprises soaking the flax fibers in a flowing detergent at a temperature of 30 to 40° C. for 20 to 25 minutes, and rinsing the flax fibers with clean water for 3 to 5 times after the soaking is completed.
5. The high-elastic wrinkle-resistant linen antibacterial fabric according to claim 2, characterized in that: During the secondary heat preservation, the mixed solution is placed in a pressure container, and nitrogen is filled into the pressure container to make the pressure in the pressure container reach 0.6-0.8 MPa.
6. A method for preparing a highly elastic and wrinkle-resistant linen antibacterial fabric, used for preparing a highly elastic and wrinkle-resistant linen antibacterial fabric as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1, feeding the modified flax fiber, polyester fiber and polyacrylonitrile fiber into a blending machine according to a proportion, and blending them in the blending machine to obtain mixed spinning; Step 2: Weaving the mixed yarn to obtain linen fabric, and then performing antibacterial finishing on the linen fabric to obtain antibacterial fabric.
7. The method for preparing a highly elastic and wrinkle-resistant linen antibacterial fabric according to claim 6, characterized in that: The antibacterial finishing method comprises: heating the antibacterial finishing liquid to 30-40° C., then dipping the linen fabric into the antibacterial finishing liquid, taking out the linen fabric for air drying every 3-5 minutes during the dipping process, the single air drying time being 15-20 minutes, the wind speed being 10-12 m / s, until the antibacterial fabric is obtained after air drying 2-4 times, and the temperature of the antibacterial finishing liquid is increased by 5-8° C. after each air drying.
8. The method for preparing a highly elastic and wrinkle-resistant linen antibacterial fabric according to claim 7, characterized in that: The components of the antibacterial finishing liquid include, by weight: 15-25 parts of sodium lauryl sulfate, 5-10 parts of disodium hydrogen phosphate, 3-8 parts of silver nitrate, 5-10 parts of sodium salicylate, 2-4 parts of polydimethylsiloxane, and 50-75 parts of deionized water.
Citation Information
Patent Citations
Method for preparing antibacterial agent achieving antibacterial effect on decorative textile fabric
CN101798324A
Preparation method of antibacterial blended yarn for underwear
CN110373762A
Preparation method of linen fiber antibacterial blended fabric
CN110959938A
Antibacterial fabric and production process thereof
CN116005454A
Light and thin skin-friendly fabric
CN117449099A