Manufacturing method of composite fiber hot-rolled non-woven fabric

Through the production method of composite fiber hot-rolled non-woven fabrics, combined with modified fibers and steam injection technology, the problem of insufficient mechanical properties of non-woven fabrics is solved, and high mechanical properties and environmental protection are improved.

CN118792806APending Publication Date: 2024-10-18JIAXING SHENXIN NON WOVEN FABRIC CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410981960.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-19
Filing Date
2024-07-22
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing non-woven fabrics have deficiencies in improving mechanical properties and are difficult to meet the high requirements for softness, bulk and mechanical properties at the same time.

Method used

Using the production method of composite fiber hot-rolled non-woven fabric, by mixing modified polypropylene fiber, modified mugwort fiber, cotton fiber and polyester fiber, and forming a macromolecular network structure through hot rolling and steam injection technology to improve the mechanical properties and antioxidant and antibacterial properties.

Benefits of technology

The mechanical properties and health and environmental protection of non-woven fabrics are significantly improved. Through the synergistic effect of modified fibers and additives, the mechanical properties and antibacterial effects of the fibers are enhanced, meeting high mechanical performance and environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792806A_ABST
    Figure CN118792806A_ABST
Patent Text Reader

Abstract

The invention is applicable to the technical field of non-woven fabrics, and provides a manufacturing method of a composite fiber hot-rolled non-woven fabric, which comprises the following steps: weighing the following raw materials: modified polypropylene fiber, ES adhesive fiber, modified wormwood fiber, cotton fiber and polyester fiber; the raw materials are mixed and opened to prepare mixed fibers, and the mixed fibers are carded into non-woven fabric grey cloth; the non-woven fabric grey cloth is pulled to a spunlace area for forward and reverse spunlace; mangling the spunlaced non-woven fabric grey cloth by a mangling machine and then drying; according to the manufacturing method of the composite fiber hot-rolled non-woven fabric, the mechanical performance of the non-woven fabric is improved by adding the modified polypropylene fibers, the non-woven fabric is healthy and environmentally friendly by adding the modified wormwood fibers, the antibacterial effect of the non-woven fabric is improved, and the composite fiber hot-rolled non-woven fabric is obtained. And the mechanical property is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of non-woven fabrics, and in particular relates to a method for manufacturing composite fiber hot-rolled non-woven fabrics. Background Art

[0002] Non-woven fabrics, also known as non-woven fabrics, are made of directional or random fibers. They are called non-woven fabrics because they have the appearance and certain properties of cloth. In recent years, as people's quality requirements for various non-woven products have become higher and higher, manufacturers have also put forward higher requirements on various performance indicators of non-woven fabrics. The existing non-woven fabrics have good softness and fluffiness, but how to improve the mechanical properties of non-woven fabrics at the same time is a focus of current research. Summary of the invention

[0003] The present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, aiming to solve the above-mentioned problem.

[0004] The present invention is achieved by a method for preparing a composite fiber hot-rolled non-woven fabric, comprising the following steps: Weigh the following raw materials in parts by weight: 50-60 parts of modified polypropylene fiber, 10-20 parts of ES bonding fiber, 20-30 parts of modified wormwood fiber, 10-16 parts of cotton fiber, and 6-12 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The nonwoven fabric is obtained by hot rolling the dried nonwoven fabric through a hot rolling mill, wherein the temperature of the hot rolling roller is 100-120°C and the pressure of the hot rolling roller is 0.4-1.0 kg / cm 2 .

[0005] Preferably, the following raw materials are weighed in parts by weight: 52-58 parts of modified polypropylene fiber, 12-18 parts of ES bonding fiber, 23-27 parts of modified wormwood fiber, 11-155 parts of cotton fiber, and 8-10 parts of polyester fiber.

[0006] Preferably, the following raw materials are weighed in parts by weight: 55 parts of modified polypropylene fiber, 15 parts of ES bonding fiber, 25 parts of modified wormwood fiber, 13 parts of cotton fiber, and 9 parts of polyester fiber.

[0007] Preferably, the preparation method of the modified polypropylene fiber is as follows: 80-100 parts of polypropylene, 4-8 parts of polypropylene elastomer, 5-9 parts of modified gas silicon, and 6-12 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cooling air volume for spinning and cooling is 8000-10000m 3 / min, temperature is 12-20℃, humidity is 65%, wind speed is 1-2m / s; air flow pressure of air flow stretching is 0.05-0.1MPa, drafting air flow speed is 3000-5000m / min, and yarn speed is 2000-4000m / min.

[0008] Preferably, the preparation method of the modified gas silica is as follows: after soaking the gas phase silica in a hydrochloric acid solution with a concentration of 30-40% at 100-120°C for 1-2h, the pH value is adjusted to 6-8, and the gas phase silica after drying is placed under tetramethyltetravinylcyclotetrasiloxane vapor, and contacted and reacted in a fluidized bed for 40-60min to obtain the modified gas silica. The modified gas silica used in the present invention can be evenly dispersed in the system, improve the bonding ability of the gas phase silica with the system, is conducive to forming a network structure, and can improve the mechanical properties of polypropylene fibers.

[0009] Preferably, the preparation method of the modified lignin is as follows: by weight, 10-15 parts of lignin are mixed with 10-20 parts of a 1-3% sodium hydroxide solution, 10-20 parts of a 75% ethanol solution and 5-8 parts of allyl chloride, reacted at 40-60° C. for 30-50 minutes, dried at 80-100° C., washed the product with deionized water 3 times, added the washed product to 50-60 parts of a 30-50wt% gluconic acid solution; heated to 120-160° C., reacted for 1-3 hours, and obtained modified lignin; the modified lignin used in the present invention can promote the formation of polypropylene fiber crystals and improve the mechanical properties of polypropylene fibers.

[0010] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 10-30 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 40-60°C for 20-40 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 25-30°C for 2-5 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until colorless, and finally filter and dry it to obtain modified wormwood fiber. Under heating conditions, the hydrogen peroxide in the sponge decomposes to produce oxygen, and the oxygen enters the wormwood fiber upward to expand the pores, making the wormwood fiber more dense and porous, and having a larger specific surface area. During the fermentation process, the bacterial cellulose grows into the bamboo charcoal fiber to form an interlaced interpenetrating network with it, further improving the mechanical properties of the wormwood fiber.

[0011] Preferably, the preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 25-30°C, the stirring speed is 200-240r / min, and the culture time is 24-36h to obtain seed liquid; the seed liquid with a volume of 10-15% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid.

[0012] Preferably, after combing into a non-woven fabric, a modified polyethylene glycol solution with a concentration of 20-30% and a tea polyphenol solution with a concentration of 10-20% are prepared, and the modified polyethylene glycol solution and the tea polyphenol solution are heated at 100-120°C respectively to generate steam, and then the steam is sprayed onto the non-woven fabric for 20-30 minutes, and the steam fully enters the non-woven fabric. By spraying the steam generated by the modified polyethylene glycol solution onto the non-woven fabric, the modified polyethylene glycol forms a macromolecular network structure in the non-woven fabric, thereby further improving the mechanical properties of the non-woven fabric. By spraying the steam generated by the tea polyphenol solution onto the non-woven fabric, the antioxidant and antibacterial properties of the non-woven fabric are further improved.

[0013] Preferably, the preparation method of the modified polyethylene glycol is as follows: 12-16 parts of polyethylene glycol are taken by weight, added to 40-50 parts of water, and then 2-4 parts of 3-amino-1,2-propylene glycol and 1-5 parts of diethylamine are added, the temperature is raised to 80-90° C. and stirred for 1-2 hours, extracted with dichloromethane, precipitated with anhydrous ether, and vacuum dried to obtain the modified polyethylene glycol, and the reaction activity of the polyethylene glycol is improved by grafting amino groups on the ends of the polyethylene glycol.

[0014] Compared with the prior art, the embodiments of the present application have the following beneficial effects: The method for preparing the composite fiber hot-rolled non-woven fabric provided by the present invention improves the mechanical properties of the non-woven fabric by adding modified polypropylene fiber, and is healthy and environmentally friendly by adding modified wormwood fiber, and has the function of improving the antibacterial effect of the non-woven fabric and having good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a flow chart of a method for making a composite fiber hot-rolled non-woven fabric provided by Examples 1-5 of the present invention; Figure 2 It is a flow chart of a method for making a composite fiber hot-rolled non-woven fabric provided in Examples 6-8 of the present invention. DETAILED DESCRIPTION

[0016] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.

[0017] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments. Example 1

[0018] The embodiment of the present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, such as Figure 1 As shown, the following steps are included: Weigh the following raw materials in parts by weight: 50 parts of modified polypropylene fiber, 10 parts of ES bonding fiber, 20 parts of modified wormwood fiber, 10 parts of cotton fiber, and 6 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The dried nonwoven fabric is hot-rolled by a hot rolling mill to obtain a nonwoven fabric, wherein the temperature of the hot rolling roller is 100°C and the pressure of the hot rolling roller is 0.4 kg / cm 2 .

[0019] The preparation method of the modified polypropylene fiber is as follows: 80 parts of polypropylene, 4 parts of polypropylene elastomer, 5 parts of modified gas silicon and 6 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cooling air volume for spinning and cooling is 8000m 3 / min, temperature is 12℃, humidity is 65%, wind speed is 1m / s; air flow pressure of air flow stretching is 0.05MPa, drawing air flow speed is 3000m / min, and yarn speed is 2000m / min.

[0020] Specifically, the preparation method of the modified gas silicon is as follows: the gas phase silica is soaked in a 30% hydrochloric acid solution at 100°C for 1 hour, the pH value is adjusted to 6, and the gas phase silica is dried at 80°C for 30 minutes; the gas phase silica after the drying treatment is placed in tetramethyltetravinylcyclotetrasiloxane vapor, contacted and reacted in a fluidized bed for 40 minutes to obtain the modified gas silicon.

[0021] In this embodiment, the preparation method of the modified lignin is as follows: by weight, 10 parts of lignin are mixed with 10 parts of 1% sodium hydroxide solution, 10 parts of 75% ethanol solution and 5 parts of allyl chloride, reacted at 40°C for 30 minutes, dried at 80°C, the product was washed with deionized water 3 times, and the washed product was added to 50 parts of 30wt% gluconic acid solution; heated to 120°C, reacted for 1 hour, and obtained modified lignin.

[0022] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 10 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 40°C for 20 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 25°C for 2 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

[0023] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 25°C, the stirring speed is 200r / min, and the culture time is 24h to obtain seed liquid; the seed liquid with a volume of 10% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid. Example 2

[0024] The embodiment of the present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, such as Figure 1 As shown, the following steps are included: Weigh the following raw materials in parts by weight: 52 parts of modified polypropylene fiber, 12 parts of ES bonding fiber, 23 parts of modified wormwood fiber, 11 parts of cotton fiber, and 8 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The dried nonwoven fabric is hot-rolled by a hot rolling mill to obtain a nonwoven fabric, wherein the temperature of the hot rolling roller is 100°C and the pressure of the hot rolling roller is 0.4 kg / cm 2 .

[0025] The preparation method of the modified polypropylene fiber is as follows: 80 parts of polypropylene, 4 parts of polypropylene elastomer, 5 parts of modified gas silicon and 6 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cooling air volume for spinning and cooling is 8000m 3 / min, temperature is 12℃, humidity is 65%, wind speed is 1m / s; air flow pressure of air flow stretching is 0.05MPa, drawing air flow speed is 3000m / min, and yarn speed is 2000m / min.

[0026] Specifically, the preparation method of the modified gas silicon is as follows: the gas phase silica is soaked in a 30% hydrochloric acid solution at 100°C for 1 hour, the pH value is adjusted to 6, and the gas phase silica is dried at 80°C for 30 minutes; the gas phase silica after the drying treatment is placed in tetramethyltetravinylcyclotetrasiloxane vapor, contacted and reacted in a fluidized bed for 40 minutes to obtain the modified gas silicon.

[0027] In this embodiment, the preparation method of the modified lignin is as follows: by weight, 10 parts of lignin are mixed with 10 parts of 1% sodium hydroxide solution, 10 parts of 75% ethanol solution and 5 parts of allyl chloride, reacted at 40°C for 30 minutes, dried at 80°C, the product was washed with deionized water 3 times, and the washed product was added to 50 parts of 30wt% gluconic acid solution; heated to 120°C, reacted for 1 hour, and obtained modified lignin.

[0028] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 10 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 40°C for 20 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 25°C for 2 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

[0029] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 25°C, the stirring speed is 200r / min, and the culture time is 24h to obtain seed liquid; the seed liquid with a volume of 10% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid. Example 3

[0030] The embodiment of the present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, such as Figure 1 As shown, the following steps are included: Weigh the following raw materials in parts by weight: 55 parts of modified polypropylene fiber, 15 parts of ES bonding fiber, 25 parts of modified wormwood fiber, 13 parts of cotton fiber, and 9 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The dried nonwoven fabric is hot-rolled by a hot rolling mill to obtain a nonwoven fabric, wherein the temperature of the hot rolling roller is 110°C and the pressure of the hot rolling roller is 0.7 kg / cm 2 .

[0031] The preparation method of the modified polypropylene fiber is as follows: 90 parts of polypropylene, 6 parts of polypropylene elastomer, 7 parts of modified gas silicon and 9 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cold air volume for spinning cooling is 9000m 3 / min, temperature is 16℃, humidity is 65%, wind speed is 1.5m / s; air flow pressure of air flow stretching is 0.075MPa, drawing air flow speed is 4000m / min, and yarn speed is 3000m / min.

[0032] Specifically, the preparation method of the modified gas silicon is as follows: the gas phase silica is soaked in a 35% hydrochloric acid solution at 100-120°C for 1.5 hours, the pH value is adjusted to 7, and the gas phase silica is dried at 90°C for 40 minutes; the gas phase silica after the drying treatment is placed in tetramethyltetravinylcyclotetrasiloxane vapor, contacted and reacted in a fluidized bed for 50 minutes to obtain the modified gas silicon.

[0033] In this embodiment, the preparation method of the modified lignin is as follows: by weight, 12.5 parts of lignin are mixed with 15 parts of 2% sodium hydroxide solution, 15 parts of 75% ethanol solution and 6.5 parts of propylene chloride, reacted at 50°C for 40 minutes, dried at 90°C, the product was washed with deionized water 3 times, and the washed product was added to 55 parts of 40wt% gluconic acid solution; heated to 140°C, reacted for 2 hours, and obtained modified lignin.

[0034] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 20 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 550°C for 30 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 28°C for 3.5 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

[0035] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 28°C, the stirring speed is 220r / min, and the culture time is 30h to obtain seed liquid; the seed liquid with a volume of 13% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid. Example 4

[0036] The embodiment of the present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, such as Figure 1 As shown, the following steps are included: Weigh the following raw materials in parts by weight: 58 parts of modified polypropylene fiber, 18 parts of ES bonding fiber, 27 parts of modified wormwood fiber, 155 parts of cotton fiber, and 10 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The dried nonwoven fabric is hot-rolled by a hot rolling mill to obtain a nonwoven fabric, wherein the temperature of the hot rolling roller is 120°C and the pressure of the hot rolling roller is 1.0 kg / cm2 .

[0037] The preparation method of the modified polypropylene fiber is as follows: 100 parts of polypropylene, 8 parts of polypropylene elastomer, 9 parts of modified gas silicon, and 12 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cooling air volume for spinning and cooling is 10000m 3 / min, temperature is 20℃, humidity is 65%, wind speed is 2m / s; air flow pressure of air flow stretching is 0.1MPa, drawing air flow speed is 5000m / min, and yarn speed is 4000m / min.

[0038] Specifically, the preparation method of the modified gas silicon is as follows: after soaking the gas-phase silica in a 40% hydrochloric acid solution at 120°C for 2 hours, the pH value is adjusted to 8, and the gas-phase silica is dried at 100°C for 50 minutes; the gas-phase silica after the drying treatment is placed in tetramethyltetravinylcyclotetrasiloxane vapor, contacted and reacted in a fluidized bed for 60 minutes to obtain the modified gas silicon.

[0039] In this embodiment, the preparation method of the modified lignin is as follows: by weight, 15 parts of lignin are mixed with 20 parts of 3% sodium hydroxide solution, 20 parts of 75% ethanol solution and 8 parts of allyl chloride, reacted at 60°C for 50 minutes, dried at 100°C, the product was washed with deionized water 3 times, and the washed product was added to 60 parts of 50wt% gluconic acid solution; heated to 160°C, reacted for 3 hours, and obtained modified lignin.

[0040] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 30 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 60°C for 40 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 30°C for 5 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

[0041] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 30°C, the stirring speed is 240r / min, and the culture time is 36h to obtain seed liquid; the seed liquid with a volume of 15% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid. Example 5

[0042] The embodiment of the present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, such as Figure 1 As shown, the following steps are included: Weigh the following raw materials in parts by weight: 60 parts of modified polypropylene fiber, 20 parts of ES bonding fiber, 30 parts of modified wormwood fiber, 16 parts of cotton fiber, and 12 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The dried nonwoven fabric is hot-rolled by a hot rolling mill to obtain a nonwoven fabric, wherein the temperature of the hot rolling roller is 120°C and the pressure of the hot rolling roller is 1.0 kg / cm 2 .

[0043] The preparation method of the modified polypropylene fiber is as follows: 100 parts of polypropylene, 8 parts of polypropylene elastomer, 9 parts of modified gas silicon, and 12 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cooling air volume for spinning and cooling is 10000m 3 / min, temperature is 20℃, humidity is 65%, wind speed is 2m / s; air flow pressure of air flow stretching is 0.1MPa, drawing air flow speed is 5000m / min, and yarn speed is 4000m / min.

[0044] Specifically, the preparation method of the modified gas silicon is as follows: after soaking the gas-phase silica in a 40% hydrochloric acid solution at 120°C for 2 hours, the pH value is adjusted to 8, and the gas-phase silica is dried at 100°C for 50 minutes; the gas-phase silica after the drying treatment is placed in tetramethyltetravinylcyclotetrasiloxane vapor, contacted and reacted in a fluidized bed for 60 minutes to obtain the modified gas silicon.

[0045] In this embodiment, the preparation method of the modified lignin is as follows: by weight, 15 parts of lignin are mixed with 20 parts of 3% sodium hydroxide solution, 20 parts of 75% ethanol solution and 8 parts of allyl chloride, reacted at 60°C for 50 minutes, dried at 100°C, the product was washed with deionized water 3 times, and the washed product was added to 60 parts of 50wt% gluconic acid solution; heated to 160°C, reacted for 3 hours, and obtained modified lignin.

[0046] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 30 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 60°C for 40 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 30°C for 5 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

[0047] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 30°C, the stirring speed is 240r / min, and the culture time is 36h to obtain seed liquid; the seed liquid with a volume of 15% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid. Example 6

[0048] The embodiment of the present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, such as Figure 2 As shown, the following steps are included: Weigh the following raw materials in parts by weight: 55 parts of modified polypropylene fiber, 15 parts of ES bonding fiber, 25 parts of modified wormwood fiber, 13 parts of cotton fiber, and 9 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; A modified polyethylene glycol solution with a concentration of 20% and a tea polyphenol solution with a concentration of 10% were prepared, and the modified polyethylene glycol solution and the tea polyphenol solution were heated at 100°C respectively to generate steam, and then the steam was sprayed onto the non-woven fabric for 20 minutes, and the steam fully entered the non-woven fabric; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The dried nonwoven fabric is hot-rolled by a hot rolling mill to obtain a nonwoven fabric, wherein the temperature of the hot rolling roller is 110°C and the pressure of the hot rolling roller is 0.7 kg / cm 2 .

[0049] The preparation method of the modified polypropylene fiber is as follows: 90 parts of polypropylene, 6 parts of polypropylene elastomer, 7 parts of modified gas silicon and 9 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cold air volume for spinning cooling is 9000m 3 / min, temperature is 16℃, humidity is 65%, wind speed is 1.5m / s; air flow pressure of air flow stretching is 0.075MPa, drawing air flow speed is 4000m / min, and yarn speed is 3000m / min.

[0050] Specifically, the preparation method of the modified gas silicon is as follows: the gas phase silica is soaked in a 35% hydrochloric acid solution at 100-120°C for 1.5 hours, the pH value is adjusted to 7, and the gas phase silica is dried at 90°C for 40 minutes; the gas phase silica after the drying treatment is placed in tetramethyltetravinylcyclotetrasiloxane vapor, contacted and reacted in a fluidized bed for 50 minutes to obtain the modified gas silicon.

[0051] In this embodiment, the preparation method of the modified lignin is as follows: by weight, 12.5 parts of lignin are mixed with 15 parts of 2% sodium hydroxide solution, 15 parts of 75% ethanol solution and 6.5 parts of propylene chloride, reacted at 50°C for 40 minutes, dried at 90°C, the product was washed with deionized water 3 times, and the washed product was added to 55 parts of 40wt% gluconic acid solution; heated to 140°C, reacted for 2 hours, and obtained modified lignin.

[0052] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 20 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 550°C for 30 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 28°C for 3.5 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

[0053] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 28°C, the stirring speed is 220r / min, and the culture time is 30h to obtain seed liquid; the seed liquid with a volume of 13% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid.

[0054] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: 12 parts of polyethylene glycol are taken by weight, added to 40 parts of water, and then 2 parts of 3-amino-1,2-propylene glycol and 1 part of diethylamine are added, the temperature is raised to 80° C. and stirred for 1 hour, extracted with dichloromethane, precipitated with anhydrous ether, and vacuum dried to obtain the modified polyethylene glycol. Example 7

[0055] The embodiment of the present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, such as Figure 2 As shown, the following steps are included: Weigh the following raw materials in parts by weight: 55 parts of modified polypropylene fiber, 15 parts of ES bonding fiber, 25 parts of modified wormwood fiber, 13 parts of cotton fiber, and 9 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; A modified polyethylene glycol solution with a concentration of 25% and a tea polyphenol solution with a concentration of 15% were prepared, and the modified polyethylene glycol solution and the tea polyphenol solution were heated at 110°C respectively to generate steam, and then the steam was sprayed onto the non-woven fabric for 25 minutes, and the steam fully entered the non-woven fabric; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The dried nonwoven fabric is hot-rolled by a hot rolling mill to obtain a nonwoven fabric, wherein the temperature of the hot rolling roller is 110°C and the pressure of the hot rolling roller is 0.7 kg / cm 2 .

[0056] The preparation method of the modified polypropylene fiber is as follows: 90 parts of polypropylene, 6 parts of polypropylene elastomer, 7 parts of modified gas silicon and 9 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cold air volume for spinning cooling is 9000m 3 / min, temperature is 16℃, humidity is 65%, wind speed is 1.5m / s; air flow pressure of air flow stretching is 0.075MPa, drawing air flow speed is 4000m / min, and yarn speed is 3000m / min.

[0057] Specifically, the preparation method of the modified gas silicon is as follows: the gas phase silica is soaked in a 35% hydrochloric acid solution at 100-120°C for 1.5 hours, the pH value is adjusted to 7, and the gas phase silica is dried at 90°C for 40 minutes; the gas phase silica after the drying treatment is placed in tetramethyltetravinylcyclotetrasiloxane vapor, contacted and reacted in a fluidized bed for 50 minutes to obtain the modified gas silicon.

[0058] In this embodiment, the preparation method of the modified lignin is as follows: by weight, 12.5 parts of lignin are mixed with 15 parts of 2% sodium hydroxide solution, 15 parts of 75% ethanol solution and 6.5 parts of propylene chloride, reacted at 50°C for 40 minutes, dried at 90°C, the product was washed with deionized water 3 times, and the washed product was added to 55 parts of 40wt% gluconic acid solution; heated to 140°C, reacted for 2 hours, and obtained modified lignin.

[0059] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 20 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 550°C for 30 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 28°C for 3.5 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

[0060] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 28°C, the stirring speed is 220r / min, and the culture time is 30h to obtain seed liquid; the seed liquid with a volume of 13% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid.

[0061] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: 14 parts of polyethylene glycol are taken by weight, added to 45 parts of water, and then 3 parts of 3-amino-1,2-propylene glycol and 3 parts of diethylamine are added, the temperature is raised to 85° C. and stirred for 1.5 hours, extracted with dichloromethane, precipitated with anhydrous ether, and vacuum dried to obtain the modified polyethylene glycol. Example 8

[0062] The embodiment of the present invention provides a method for manufacturing a composite fiber hot-rolled non-woven fabric, such as Figure 2 As shown, the following steps are included: Weigh the following raw materials in parts by weight: 55 parts of modified polypropylene fiber, 15 parts of ES bonding fiber, 25 parts of modified wormwood fiber, 13 parts of cotton fiber, and 9 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; A modified polyethylene glycol solution with a concentration of 30% and a tea polyphenol solution with a concentration of 20% were prepared, and the modified polyethylene glycol solution and the tea polyphenol solution were heated at 120°C respectively to generate steam, and then the steam was sprayed onto the non-woven fabric for 30 minutes, and the steam fully entered the non-woven fabric; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The dried nonwoven fabric is hot-rolled by a hot rolling mill to obtain a nonwoven fabric, wherein the temperature of the hot rolling roller is 110°C and the pressure of the hot rolling roller is 0.7 kg / cm 2 .

[0063] The preparation method of the modified polypropylene fiber is as follows: 90 parts of polypropylene, 6 parts of polypropylene elastomer, 7 parts of modified gas silicon and 9 parts of modified lignin are weighed and mixed, melted and heated, filtered and distributed, and then spun and cooled, and air flow stretched to obtain the modified polypropylene fiber; wherein the cold air volume for spinning cooling is 9000m 3 / min, temperature is 16℃, humidity is 65%, wind speed is 1.5m / s; air flow pressure of air flow stretching is 0.075MPa, drawing air flow speed is 4000m / min, and yarn speed is 3000m / min.

[0064] Specifically, the preparation method of the modified gas silicon is as follows: the gas phase silica is soaked in a 35% hydrochloric acid solution at 100-120°C for 1.5 hours, the pH value is adjusted to 7, and the gas phase silica is dried at 90°C for 40 minutes; the gas phase silica after the drying treatment is placed in tetramethyltetravinylcyclotetrasiloxane vapor, contacted and reacted in a fluidized bed for 50 minutes to obtain the modified gas silicon.

[0065] In this embodiment, the preparation method of the modified lignin is as follows: by weight, 12.5 parts of lignin are mixed with 15 parts of 2% sodium hydroxide solution, 15 parts of 75% ethanol solution and 6.5 parts of propylene chloride, reacted at 50°C for 40 minutes, dried at 90°C, the product was washed with deionized water 3 times, and the washed product was added to 55 parts of 40wt% gluconic acid solution; heated to 140°C, reacted for 2 hours, and obtained modified lignin.

[0066] Preferably, the preparation method of the modified wormwood fiber is as follows: take a sponge, soak it in hydrogen peroxide for 20 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 550°C for 30 minutes, then take out the wormwood fiber and put it into a culture vessel and inject bacterial cellulose fermentation liquid, wrap it, and culture it at 28°C for 3.5 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

[0067] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into the culture liquid, the temperature is 28°C, the stirring speed is 220r / min, and the culture time is 30h to obtain seed liquid; the seed liquid with a volume of 13% of the culture liquid is added to the culture liquid, mixed and set aside to obtain bacterial cellulose fermentation liquid.

[0068] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: 16 parts of polyethylene glycol are taken by weight, added to 50 parts of water, and then 4 parts of 3-amino-1,2-propylene glycol and 5 parts of diethylamine are added, the temperature is raised to 90° C. and stirred for 2 hours, extracted with dichloromethane, precipitated with anhydrous ether, and vacuum dried to obtain the modified polyethylene glycol.

[0069] Comparative Example 1 Compared with Example 3, the modified polypropylene fiber is replaced by ordinary polypropylene fiber.

[0070] Comparative Example 2 Compared with Example 3, the modified wormwood fiber is replaced by ordinary wormwood fiber.

[0071] Comparative Example 3 Compared with Example 3, the modified gas silica in the modified polypropylene fiber raw material is replaced with ordinary gas silica.

[0072] Comparative Example 4 Compared with Example 3, the modified lignin in the modified polypropylene fiber raw material is replaced with ordinary lignin.

[0073] Comparative Example 5 Compared with Example 3, the modified gas silica in the modified polypropylene fiber raw material is replaced by ordinary gas silica and the modified lignin is replaced by ordinary lignin.

[0074] Comparative Example 6 Compared with Example 7, the modified polyethylene glycol was replaced with ordinary polyethylene glycol.

[0075] The nonwoven fabrics of Examples 1-8 and Comparative Examples 1-6 were subjected to performance tests, wherein longitudinal strength, longitudinal elongation at break, transverse strength, and transverse elongation at break were tested according to standard GB / T 12914-2018, and the results are shown in the following table: Group Longitudinal strength (N / 5cm) Longitudinal elongation at break (%) Transverse strength (N / 5cm) Transverse elongation at break (%) Example 1 55.5 77.2 30.3 75.8 Example 2 55.6 77.5 30.5 76.1 Example 3 55.9 77.6 30.8 76.3 Example 4 55.7 77.5 30.6 76.2 Example 5 55.5 77.3 30.5 75.9 Example 6 59.6 81.2 34.2 80.1 Example 7 59.9 81.5 34.6 80.3 Example 8 59.8 81.4 34.4 80.1 Comparative Example 1 45.3 65.8 22.3 64.5 Comparative Example 2 48.2 68.9 25.7 67.3 Comparative Example 3 50.2 70.8 26.5 69.5 Comparative Example 4 50.5 71.5 26.9 70.1 Comparative Example 5 47.4 67.6 24.6 66.2 Comparative Example 6 57.2 79.7 32.5 77.8 In summary, the composite fiber hot-rolled non-woven fabric provided by the present invention has excellent mechanical properties. The mechanical properties of the non-woven fabric are improved by adding modified polypropylene fiber. By adding modified wormwood fiber, it is healthy and environmentally friendly, and the mechanical properties of the non-woven fabric are improved. In particular, by adding modified gas silica and modified lignin to the modified polypropylene fiber, the two have a synergistic effect, which further improves the mechanical properties of the non-woven fabric. Steam is generated by a modified polyethylene glycol solution with a concentration of 30% and a tea polyphenol solution with a concentration of 20%, and the steam is sprayed onto the non-woven fabric, which further improves the mechanical properties of the non-woven fabric.

[0076] It should be noted that, for the above embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the described order of actions, because according to the present invention, some steps may be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present invention.

[0077] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.

Claims

1. A method for producing a composite fiber hot-rolled nonwoven fabric, characterized in that: The steps include: Weigh the following raw materials in parts by weight: 50-60 parts of modified polypropylene fiber, 10-20 parts of ES bonding fiber, 20-30 parts of modified wormwood fiber, 10-16 parts of cotton fiber, and 6-12 parts of polyester fiber; The raw materials are mixed and opened to make mixed fibers, and the mixed fibers are combed to make non-woven fabrics; The nonwoven fabric is pulled to the spunlace area for positive and negative spunlace; The non-woven fabric after spunlaced is squeezed through a squeezer and then dried; The nonwoven fabric is obtained by hot-rolling the dried nonwoven fabric through a hot-rolling machine.

2. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 1, characterized in that: The method comprises the following steps: weighing the following raw materials in parts by weight: 52-58 parts of modified polypropylene fiber, 12-18 parts of ES bonding fiber, 23-27 parts of modified wormwood fiber, 11-155 parts of cotton fiber and 8-10 parts of polyester fiber.

3. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 2, characterized in that: The method comprises the following steps: weighing the following raw materials in parts by weight: 55 parts of modified polypropylene fiber, 15 parts of ES bonding fiber, 25 parts of modified wormwood fiber, 13 parts of cotton fiber and 9 parts of polyester fiber.

4. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 1, characterized in that: The preparation method of the modified polypropylene fiber is as follows: 80-100 parts of polypropylene, 4-8 parts of polypropylene polymer, 5-9 parts of modified gas silica and 6-12 parts of modified lignin are weighed and mixed, melt-heated, filtered and distributed, and then spun and cooled, and air-stretched to obtain the modified polypropylene fiber.

5. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 4, characterized in that: The preparation method of the modified gas silicon is as follows: after soaking the gas phase silicon dioxide in a hydrochloric acid solution with a concentration of 30-40% at 100-120° C. for 1-2 hours, adjusting the pH value to 6-8, and drying the gas phase silicon dioxide at 80-100° C. for 30-50 minutes; placing the dried gas phase silicon dioxide under tetramethyltetravinylcyclotetrasiloxane vapor, contacting and reacting in a fluidized bed for 40-60 minutes, thereby obtaining the modified gas silicon.

6. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 4, characterized in that: The preparation method of the modified lignin is as follows: by weight, 10-15 parts of lignin are mixed with 10-20 parts of a sodium hydroxide solution with a concentration of 1-3%, 10-20 parts of an ethanol solution with a concentration of 75% and 5-8 parts of allyl chloride, reacting at 40-60° C. for 30-50 minutes, drying at 80-100° C., washing the product with deionized water for 3 times, adding the washed product to 50-60 parts of a gluconic acid solution with a concentration of 30-50wt%; heating to 120-160° C., reacting for 1-3 hours, and obtaining the modified lignin.

7. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 1, characterized in that: The preparation method of the modified wormwood fiber is as follows: take a sponge, immerse it in hydrogen peroxide for 10-30 minutes, then spread the wormwood fiber on the sponge, put it in a container, heat it to 40-60°C for 20-40 minutes, then take out the wormwood fiber, put it into a culture vessel, inject bacterial cellulose fermentation liquid, wrap it, and culture it at 25-30°C for 2-5 days, rinse the culture product with deionized water, remove the residual culture liquid, soak it with deionized water until it is colorless, and finally filter and dry it to obtain the modified wormwood fiber.

8. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 7, characterized in that: The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into a culture liquid, the temperature is 25-30°C, the stirring speed is 200-240r / min, and the culture time is 24-36h to obtain a seed liquid; the seed liquid with a volume of 10-15% of the culture liquid is added to the culture liquid, mixed and set aside, to obtain a bacterial cellulose fermentation liquid.

9. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 1, characterized in that: After combing into non-woven fabric, prepare a modified polyethylene glycol solution with a concentration of 20-30% and a tea polyphenol solution with a concentration of 10-20%, heat the modified polyethylene glycol solution and the tea polyphenol solution at 100-120°C respectively to generate steam, and then spray the steam onto the non-woven fabric for 20-30 minutes, so that the steam fully enters the non-woven fabric.

10. The method for producing a composite fiber hot-rolled nonwoven fabric according to claim 9, characterized in that: The preparation method of the modified polyethylene glycol is as follows: 12-16 parts of polyethylene glycol are taken by weight, added to 40-50 parts of water, and then 2-4 parts of 3-amino-1,2-propylene glycol and 1-5 parts of diethylamine are added, the temperature is raised to 80-90° C. and stirred for 1-2 hours, extracted with dichloromethane, precipitated with anhydrous ether, and vacuum dried to obtain the modified polyethylene glycol.

Citation Information

Cited By

  • High-breathability PNK deoxidizer packaging material and production process thereof

    CN120003853A