Soft magnetic alloy particles and inductor including same

By introducing Ge and other elements into the Fe-based soft magnetic material, adjusting the content of its amorphous phase and nanocrystalline phase, and optimizing it through heat treatment, a uniform nanocrystalline structure is formed, which solves the problem of Fe-based soft magnetic material when increasing the magnetic saturation strength. It achieves high current characteristics and excellent electromagnetic properties by solving the problems of electromagnetic performance degradation and uneven nanocrystal growth.

CN118800544APending Publication Date: 2024-10-18SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410420208.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-09
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

When increasing the magnetic saturation strength (Ms) of existing Fe-based soft magnetic materials, the increase in Si content leads to a decrease in Fe metal content, deterioration of electromagnetic properties, and difficulty in maintaining high current characteristics, and local growth of nanocrystals during heat treatment leads to uneven crystal growth. .

Method used

Using soft magnetic alloy particles including Fe, Ge, Co, B, P, Cu and other elements, by adjusting the content of the amorphous phase and nanocrystalline phase of Ge to ensure that Ge(a)-Ge(c)>0, combined with heat treatment Process optimization improves crystallinity and nanocrystal size control to form a uniform nanocrystal structure.

Benefits of technology

While maintaining high magnetic saturation characteristics and improving electromagnetic properties, it ensures high current characteristics, avoids the problem of uneven nanocrystal growth, increases magnetic permeability and reduces iron loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800544A_ABST
    Figure CN118800544A_ABST
Patent Text Reader

Abstract

The invention provides a magnetically soft alloy particle and an inductor including the same. The magnetically soft alloy particles include nanocrystalline and amorphous phases, as well as Fe (iron) and Ge (germanium). The average content of Ge in the amorphous phase is Ge (a) (at%), the average content of Ge in the nanocrystalline is Ge (c) (at%), and Ge (a)-Ge (c) gt; 0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a soft magnetic alloy particle and an inductor including the soft magnetic alloy particle. Background Art

[0002] Recently, as electronic devices are reduced in size and more highly integrated, the power supply voltage is reduced, and therefore, the current value is increased to transmit the same power. Therefore, metal inductors that maintain inductor performance even at high currents have been applied, but recently, in order to ensure use at higher currents, materials with high current characteristics, that is, materials with high saturation magnetization (Ms, magnetic saturation) values ​​have been applied.

[0003] In conventional Fe-based soft magnetic materials, electromagnetic properties are improved by adjusting the content of elements such as Si to bring magnetostriction close to zero. However, when the content of Si increases, the content of metals such as Fe decreases, making it difficult to increase the Ms value.

[0004] In addition, when the content of metal such as Fe is too high, the Ms value can be increased, but there is another problem that nanocrystals grow locally during heat treatment. Therefore, this problem leads to the growth of non-uniform crystals, deteriorating the electromagnetic properties of the soft magnetic material. Summary of the invention

[0005] An aspect of an embodiment provides a soft magnetic alloy particle capable of maintaining high magnetic saturation characteristics and improving electromagnetic performance.

[0006] Another aspect of the embodiment provides an inductor using soft magnetic alloy particles.

[0007] However, the problems to be solved by the embodiments are not limited to the above-mentioned problems, and various extensions can be made within the scope of the technical ideas included in the embodiments.

[0008] According to the embodiment, the soft magnetic alloy particles include nanocrystals and amorphous phases, and include Fe (iron) and Ge (germanium), and the average content of Ge in the amorphous phase is Ge (a) (at%), the average content of Ge in the nanocrystals is Ge (c) (at%), and Ge (a) - Ge (c)>0.

[0009] The composition of the soft magnetic alloy particles can be represented by Composition Formula 1.

[0010] Composition formula 1

[0011] Fe a Co b Ge c M d

[0012] In Composition 1, a, b, c, and d respectively represent the atomic percentage contents (at%) of the corresponding elements, where 0 < a ≤ 90, 0 ≤ b ≤ 10, 0 < c ≤ 5, 0 < d ≤ 20, a + b + c + d = 100, and M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.

[0013] M may not include Si.

[0014] In the above Composition 1, c may satisfy 0.5 ≤ c ≤ 4.

[0015] In the above Composition 1, a may satisfy 70 ≤ a ≤ 80.

[0016] In the above Composition 1, b may satisfy 2 ≤ b ≤ 6.

[0017] In the above Composition 1, a and b may satisfy 75 ≤ a + b ≤ 90.

[0018] In the above Composition 1, d may satisfy 10 ≤ d ≤ 20.

[0019] Ge(a) and Ge(c) may satisfy 0.1 ≤ Ge(a) - Ge(c) ≤ 0.7.

[0020] M may include B, P, Cu, or a combination thereof.

[0021] The crystallinity of the soft magnetic alloy particles may be greater than or equal to about 59% and less than or equal to about 70%.

[0022] The average crystal size of the nanocrystals may be less than or equal to about 20 nm.

[0023] An inductor according to another embodiment includes: a body including a magnetic material, the magnetic material including soft magnetic alloy particles; a coil located in the body; and an external electrode located on an outer surface of the body. The soft magnetic alloy particles may include nanocrystals and an amorphous phase, and include Fe (iron) and Ge (germanium), and the average content of Ge in the amorphous phase is Ge(a) (at%), and the average content of Ge in the nanocrystals is Ge(c) (at%), and Ge(a) - Ge(c) > 0.

[0024] The composition of the soft magnetic alloy particles may be represented by Composition 1.

[0025] Composition 1

[0026] Fe a Co b Ge c M d

[0027] In Composition 1, a, b, c, and d respectively represent the atomic percentage contents (at%) of the corresponding elements, where 0 < a ≤ 90, 0 ≤ b ≤ 10, 0 < c ≤ 5, 0 < d ≤ 20, a + b + c + d = 100, and M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.

[0028] M may not include Si.

[0029] In the above Composition 1, c may satisfy 0.5 ≤ c ≤ 4.

[0030] The crystallinity of the soft magnetic alloy particles may be greater than or equal to about 59% and less than or equal to about 70%.

[0031] The average crystal size of the nanocrystals may be less than or equal to about 20 nm.

[0032] In the inductor according to the embodiment, the coil may include a support member, an upper coil and a lower coil respectively located on the upper surface and the lower surface of the support member, and the upper coil and the lower coil may be connected by vias penetrating the support member.

[0033] In the inductor according to another embodiment, the main body may include a molding part, a cover part on one surface of the molding part, and a core protruding from one surface of the molding part. The coil may be located between one surface of the molding part and the cover part, and the core may penetrate the coil.

[0034] In the inductor according to another embodiment, the main body may include a plurality of magnetic sheets including the magnetic material. The coil may include a plurality of conductor patterns formed in the plurality of magnetic sheets and a plurality of conductive vias penetrating the corresponding magnetic sheets in the thickness direction of the magnetic sheets to electrically connect adjacent conductor patterns.

[0035] The soft magnetic alloy particles according to the present embodiment can maintain high magnetic saturation characteristics while improving electromagnetic performance.

[0036] However, the various advantageous advantages and effects of the present invention are not limited to the above description, and will be more easily understood during the description of the specific embodiments of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 is a photograph of the soft magnetic alloy particles according to the embodiment observed with a transmission electron microscope (TEM).

[0038] Figure 2 is a photograph of conventional soft magnetic alloy particles observed with a transmission electron microscope (TEM).

[0039] Figure 3 Point quantitative analysis (top) and line analysis (bottom) of soft magnetic alloy particles according to the embodiment by TEM analysis are shown.

[0040] Figure 4 Point quantitative analysis (top) and line analysis (bottom) of soft magnetic alloy particles according to the embodiment by TEM analysis are shown.

[0041] Figure 5 is a perspective view of an inductor according to an embodiment.

[0042] Figure 6 yes Figure 5 A cross-sectional view taken along line II'.

[0043] Figure 7 yes Figure 6 Magnified view of area A.

[0044] Figure 8 is a perspective view of an inductor according to another embodiment.

[0045] Fig. 9 yes Figure 8 A cross-sectional view taken along line II-II'.

[0046] Fig.10 is a perspective view of an inductor according to another embodiment.

[0047] Fig.11 yes Fig.10 A cross-sectional view taken along line III-III'. DETAILED DESCRIPTION

[0048] Hereinafter, various embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the present invention. The drawings and descriptions are considered to be illustrative rather than restrictive in nature. Throughout the specification, the same reference numerals represent the same elements. In addition, the drawings are provided only to make the embodiments disclosed in this specification easily understood, and should not be interpreted as limiting the spirit disclosed in this specification, and it should be understood that the present invention includes all variations, equivalents and alternatives without departing from the scope and spirit of the present invention. In addition, some of the constituent elements in the drawings are enlarged, omitted or schematically shown, and the size of each constituent element does not fully reflect the actual size.

[0049] In addition, unless explicitly described to the contrary, the word “comprise” and variations such as “including” or “having”, will be understood to imply the inclusion of stated elements but not the exclusion of any other elements.

[0050] Throughout the specification, the "stacking direction" refers to the direction in which the constituent elements are stacked in sequence or the "thickness direction" perpendicular to the major surface (principal surface) of the sheet-like constituent element, and the "stacking direction" corresponds to the T-axis direction in the drawings.

[0051] In addition, the "lateral direction" refers to the direction extending parallel to the major surface (principal surface) from the edge of the sheet-like constituent element or the "plane direction", and the "lateral direction" corresponds to the L-axis direction in the drawings.

[0052] Furthermore, the W-axis direction in the drawings may be the "width direction".

[0053] Hereinafter, various embodiments and modifications will be described in detail with reference to the drawings.

[0054] Soft magnetic alloy particles

[0055] Figure 1 is a photograph of soft magnetic alloy particles according to an embodiment observed by a transmission electron microscope (TEM). For reference, the boundary between the amorphous phase portion and the nanocrystalline phase portion can be defined by dividing the portions having a contrast difference by a method such as binarizing a transmission electron microscope (TEM) image.

[0056] Refer to Figure 1 , the soft magnetic alloy particles according to the embodiment include nanocrystals and an amorphous phase, and include Fe (iron) and Ge (germanium).

[0057] The composition of the soft magnetic alloy particles according to the embodiment can be represented by Composition Formula 1.

[0058] [Composition Formula 1]

[0059] Fe a Co b Ge c M d

[0060] In Composition Formula 1, a, b, c, and d respectively represent the atomic percentage contents (at%) of the corresponding elements, 0 < a ≤ 90, 0 ≤ b ≤ 10, 0 < c ≤ 5, 0 < d ≤ 20, and a + b + c + d = 100.

[0061] M may include B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.

[0062] In the embodiment, M may include B, P, Cu, or a combination thereof.

[0063] In the embodiment, M may not include Si.

[0064] In Composition Formula 1, a represents the atomic percentage content of Fe (iron) metal, and may satisfy 70≤a≤80.

[0065] In Composition Formula 1, b represents the atomic percentage content of Co (cobalt) metal, and may satisfy 2≤b≤6.

[0066] In composition formula 1, 75≤a+b≤90. If a+b is less than 75, the saturation magnetization value is low and high current characteristics may be poor, and if a+b exceeds 90, it is difficult to control the size of nanocrystals, and thus electromagnetic properties may be poor.

[0067] In composition formula 1, 10≤d≤20.

[0068] c represents the atomic percentage content of Ge (germanium) element, and may satisfy 0.5≤c≤4. If c is less than 0.5, it is difficult to control the size of the nanocrystal, which may result in poor electromagnetic properties. If c exceeds 4, the contents of Fe and Co as metals are relatively low, making it difficult to ensure high current characteristics.

[0069] As a specific example, the composition formula 1 may be Fe 79.4 Co4Ge 0.5 B 10 P 5.5 Cu 0.6 , Fe 79.4 Co4Ge1B 10 P5C 0.6 , Fe 79.4 Co4Ge2B 10 P4C 0.6 , Fe 78.4 Co4Ge3B 10 P4C 0.6 or Fe 77.4 Co4Ge4B 10 P4C 0.6 .

[0070] In the soft magnetic alloy particles according to the embodiment, when the average content of Ge in the amorphous phase is Ge(a) (at%) and the average content of Ge in the nanocrystals is Ge(c) (at%), Ge(a)-Ge(c)>0.

[0071] Ge(a) refers to the average content (at%) of Ge based on all atoms constituting the amorphous phase of the soft magnetic alloy particles. In addition, Ge(c) refers to the average content (at%) of Ge based on all atoms constituting the nanocrystalline portion of the soft magnetic alloy particles.

[0072] Figure 3 and Figure 4The line analysis (bottom) of the point quantitative analysis (top) of the soft magnetic alloy particles by TEM analysis according to the embodiment is shown. For reference, the boundary between the amorphous phase part and the nanocrystalline part can be defined by dividing the parts with contrast difference by a method such as binarizing the transmission electron microscope (TEM) image. Figure 3 and 4 In the figure, the relatively bright part corresponds to the nanocrystals, and the relatively dark part corresponds to the amorphous phase.

[0073] Reference Figure 3 and 4 , Ge(a) and Ge(c) were measured by line analysis using EDS (Energy Dispersive X-ray Spectrometer) installed in a transmission electron microscope (TEM).

[0074] Specifically, based on the surface of any one nanocrystalline particle, in line analysis of point quantitative analysis of the inner 20 nm and outer 200 nm of the nanocrystalline particle, the maximum value of the Ge element content inside the nanocrystalline particle and the maximum value of the Ge element content in the amorphous phase are compared.

[0075] Furthermore, in order to measure the average value, the above analysis was repeated at least 5 points and the average value was calculated.

[0076] Reference Figure 3 and Figure 4 , in the case of soft magnetic alloy particles including Ge (which do not include Si and have a relatively larger atomic weight than Si), according to an embodiment, the Ge element exists more in the amorphous phase than in the nanocrystals.

[0077] In an embodiment, 0.1 (at%) ≤ Ge (a) - Ge (c) ≤ 0.7 (at%). If the Ge (a) - Ge (c) value is less than 0.1 (at%), it may become difficult to control the size of the Ge nanocrystals, resulting in poor electromagnetic properties, and if the Ge (a) - Ge (c) value exceeds 0.7 (at%), the high current characteristics may become low.

[0078] In an embodiment, the first crystallization temperature T of the soft magnetic alloy particles is x1 The second crystallization temperature T x2 The difference between the first crystallization temperature T x1 and the second crystallization temperature T x2 The difference between is less than about 100°C, then due to T x1 and T x2 The difference between them becomes smaller, making it difficult to obtain a homogeneous nanocrystalline structure, resulting in degradation of soft magnetic properties.

[0079] The amorphous phase constituting the soft magnetic alloy particles has at least two exothermic peaks indicating crystallization during a heating treatment in a DSC curve obtained by differential scanning calorimetry (DSC).

[0080] Among the exothermic peaks, the exothermic peak at the lowest temperature indicates the first crystallization in which the a-Fe primary phase crystallizes, and the subsequent exothermic peaks indicate the second crystallization in which the secondary phase of the Fe-B compound crystallizes.

[0081] In this paper, the first crystallization temperature T x1 Defined as the temperature at the intersection of the first rising tangent and the baseline, where the first rising tangent is the tangent passing through the point with the maximum positive slope in the first rising portion from the baseline of the DSC curve to the first peak (the first peak is the exothermic peak at the lowest temperature side).

[0082] In addition, the second crystallization temperature T x2 Defined as the temperature at the intersection of the second rising tangent and the baseline, where the second rising tangent is a tangent from the baseline to the point in the second rising portion of the second peak (the second peak is the exothermic peak next to the first peak) passing through the point with the maximum positive slope.

[0083] In an embodiment, the crystallinity of the soft magnetic alloy particles may be greater than or equal to about 40%, or greater than or equal to about 59%, and less than or equal to about 75%, or less than or equal to about 70%, as calculated by Formula 1. Since the crystal fraction of the soft magnetic alloy particles is increased to a level of about 60%, favorable results can be obtained in terms of high Ms.

[0084] [Formula 1]

[0085] Crystallinity (%) = [Ic / (Ic+Ia)] × 100

[0086] In Formula 1, Ic is the sum of the integrated values ​​of the scattering intensity of the crystalline peak in the X-ray diffraction analysis spectrum of the soft magnetic alloy particles, and Ia is the sum of the integrated values ​​of the scattering intensity of the amorphous halo in the X-ray diffraction analysis spectrum of the soft magnetic alloy particles.

[0087] The crystallinity of soft magnetic alloy particles can be calculated based on the curve obtained by X-ray diffraction spectrum. In the X-ray diffraction analysis spectrum, the wavelength λ and the incident angle θ of the incident X-ray are related to the lattice spacing d by 2d·sinθ=nλ, which is called the Bragg equation. Therefore, when the incident angle is determined, the lattice spacing d can be obtained.

[0088] However, since random atomic arrangements rather than regular atomic arrangements occur in amorphous materials, multiple X-ray diffractions do not appear at specific wavelengths, and a broad halo pattern appears in the region where the diffraction angle is 15° to 35°. If no peak appears at a specific angle within the diffraction angle range of 10° to 60° and a diffuse halo pattern appears, it can be determined that the amorphous material has 0% crystallinity. However, the surface of the soft magnetic alloy particles exposed to X-rays must not contain contaminants other than organic materials. As long as the result is measured under conditions where there are no factors that affect the diffraction pattern, the reliability is high.

[0089] If crystals are present in the soft magnetic alloy particles, one or more crystal peaks are present within the measured diffraction angle range. The presence of a peak means that: a peak can be identified at least with the naked eye on the X-ray diffraction spectrum, the peak has the maximum intensity on the entire vertical axis within the diffraction angle range of 2θ greater than or equal to 5° and less than or equal to 50° in the XRD pattern curve, or the waveform processing unit can clearly distinguish it from background noise and identify it as a peak.

[0090] At this time, if the crystallinity is high, the halo region is reduced, and the halo region does not exist in a material with a crystallinity of 100%. When crystals and amorphous materials are mixed, the crystallinity can be calculated by calculating the relative ratio of the area of ​​the crystallization peak and the area of ​​the halo region in a graph including intensity and diffraction angle range.

[0091] The nanocrystals of the soft magnetic alloy particles may be amorphous grains.

[0092] In an embodiment, the average crystal size of the nanocrystals of the soft magnetic alloy particles may be less than or equal to about 20 nm, for example, less than or equal to about 18 nm.

[0093] For example, the average crystal size of the nanocrystals can be calculated using the Scherer equation using the full width at half maximum (FWHM) of the main peak of the XRD pattern.

[0094] Alternatively, the average size of the nanocrystals may be obtained by measuring the maximum major axes of at least 100 nanocrystals in a scanning electron microscope (SEM) image of a cross section of the soft magnetic alloy particle to prepare a size distribution curve, and calculating D50 as the average size.

[0095] The soft magnetic alloy particles do not include Si element, but include Ge element whose atomic weight is relatively larger than Si element, and during heat treatment, Ge element can be more present in the amorphous phase than nanocrystals. Therefore, Ge element can control the size of nanocrystals to a certain size or smaller by acting as an inhibitor to prevent the growth of nanocrystals, thereby improving electromagnetic properties (such as magnetic permeability and iron loss).

[0096] In addition, by increasing the second crystallization temperature, the heat treatment process window for forming nanocrystals is improved, so that uniform nanocrystals can be obtained and the crystal fraction can be increased to a high level. Therefore, a high saturation magnetization (Ms) characteristic can be maintained.

[0097] Inductors

[0098] Hereinafter, an example of an inductor 100 including a magnetic material including the above-mentioned soft magnetic alloy particles will be described. The types of inductors may include a film type inductor, a multilayer type inductor, a wound type inductor, or a spiral type inductor, and the film type inductor will be described first.

[0099] Figure 5 is a schematic perspective view of a thin film inductor according to an embodiment, and Figure 6 yes Figure 5 A cross-sectional view taken along line I-I', Figure 6 Schematically shows Figure 5 The thin film type inductor 100 according to the embodiment includes: a body 110 including a magnetic material including soft magnetic alloy particles; a coil 130 located in the body; and external electrodes 161 and 162 located on an outer surface of the body 110 .

[0100] The body 110 forms an external appearance of the film type inductor 100 .

[0101] The main body 110 may have a hexahedral shape, including an upper surface and a lower surface opposite to each other in the stacking direction (T-axis direction) of the coil, two side surfaces opposite to each other in the length direction (L-axis direction), and a front surface and a rear surface opposite to each other in the width direction (W-axis direction), and when the printed circuit board is mounted, the lower surface (the other surface) of the main body may be a mounting surface. The corners where the surfaces intersect may be rounded by grinding or the like.

[0102] The body 110 may be formed by forming the coil 130 , stacking sheets including a magnetic material on the top and bottom of the coil 130 , and then compressing and curing the sheets.

[0103] The body 110 includes a magnetic material, and the magnetic material includes soft magnetic alloy particles according to an embodiment.

[0104] Figure 7 yes Figure 6 Magnified view of area A.

[0105] Reference Figure 6 and Figure 7, the magnetic material may include resin 20 and magnetic particles including coarse powder magnetic particles 11 or fine powder magnetic particles 12. For example, coarse powder magnetic particles 11 and fine powder magnetic particles 12 may be mixed and dispersed at a predetermined ratio using resin 20 as a matrix.

[0106] The coarse powder magnetic particles 11 may be particles having an average particle diameter of about 10 μm to about 30 μm, and the fine powder magnetic particles 12 may be particles having an average particle diameter of about 1 μm to about 10 μm.

[0107] The diameter of the magnetic particles present in the body 110 can be measured from the cross section of the body 110. Specifically, with respect to the cross section in the LT direction passing through the center of the W direction of the body 110, a plurality of regions (e.g., 10 regions) equally spaced in the T-axis direction are photographed with a scanning electron microscope, and then the diameter of the magnetic particles can be obtained using an image analysis program. In this case, since the outer region of the body 110 may be deformed or damaged due to a compression process, etc., the diameter of the magnetic particles other than the region may be measured. For example, the region corresponding to the length within about 5% or about 10% of the surface of the body 110 may be excluded.

[0108] As the magnetic particles in the present disclosure, magnetic particles used in industry can be used without limitation. For example, ferrite or a metal-based soft magnetic material can be used as the magnetic particles.

[0109] The ferrite may include known ferrites such as Mn-Zn-based ferrite, Ni-Zn-based ferrite, Ni-Zn-Cu-based ferrite, Mn-Mg-based ferrite, Ba-based ferrite, or Li-based ferrite.

[0110] The metal-based soft magnetic material may be an alloy including at least one selected from Fe, Si, Cr, Al, and Ni, and may include, for example, Fe-Si-B-Cr-based amorphous metal particles, but is not limited thereto.

[0111] In an embodiment, the magnetic particles include soft magnetic alloy particles, for example, the coarse powder magnetic particles may be soft magnetic alloy particles.

[0112] The resin may be an insulating resin, and may include epoxy resin, polyimide resin, liquid crystal polymer, or a combination thereof, but is not limited thereto.

[0113] The soft magnetic alloy particles include nanocrystalline and amorphous phases, and include Fe (iron) and Ge (germanium).

[0114] The soft magnetic alloy particles can be represented by Composition Formula 1.

[0115] [Composition formula 1]

[0116] Fe a Cob Ge c M d

[0117] In the composition formula 1, a, b, c and d represent the atomic percentage content (at%) of the corresponding elements, respectively. <a≤90、0≤b≤10、0<c≤5、0<d≤20、a+b+c+d=100。

[0118] M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S or a combination thereof.

[0119] M may include B, P, Cu, or a combination thereof, and M may not include Si.

[0120] c represents the atomic percentage content of Ge (germanium) element, and may be 0.5≤c≤4. If c is less than 0.5, it is difficult to control the size of the nanocrystal, which may result in poor electromagnetic properties. If c exceeds 4, the content of Fe and Co as metals is relatively low, making it difficult to ensure high current characteristics.

[0121] In the soft magnetic alloy particles, when the average content of Ge in the amorphous phase is Ge(a) (at%) and the average content of Ge in the nanocrystals is Ge(c) (at%), Ge(a)-Ge(c)>0.

[0122] Ge(a) refers to the average content (at%) of Ge based on all atoms constituting the amorphous phase of the soft magnetic alloy particles. In addition, Ge(c) refers to the average content (at%) of Ge based on all atoms constituting the nanocrystalline portion of the soft magnetic alloy particles.

[0123] The method of measuring Ge(a) and Ge(c) in the inductor 100 is as follows.

[0124] In a cross-sectional sample (hereinafter referred to as a "cross-sectional sample") cut from the center of the W-axis direction of the main body 110 along the L-axis direction and the T-axis direction, a line analysis of the soft magnetic alloy particles dispersed in the resin is performed using an energy dispersive X-ray spectrometer (EDS) installed in a transmission electron microscope (TEM).

[0125] For example, a cross-sectional sample of the body 110 may be prepared by adding the inductor 100 to an epoxy resin mixture and curing it, then polishing the side surfaces of the body 110 in the L-axis direction and the T-axis direction to a 1 / 2 point in the W-axis direction, and fixing and holding it in a vacuum atmosphere chamber.

[0126] Specifically, based on the surface of any one nanocrystalline particle included in the soft magnetic alloy particle, in the line analysis of the point quantitative analysis of 20nm inside and 200nm outside the nanocrystalline particle, the maximum value of the content of the Ge element inside the nanocrystalline particle and the maximum value of the content of the Ge element in the amorphous phase portion are compared. In addition, in order to measure the average value, the above analysis is repeated at at least 5 points and the average value is calculated.

[0127] The soft magnetic alloy particles may have a crystallinity greater than or equal to about 40% or greater than or equal to about 59%, and less than or equal to about 75% or less than or equal to about 70%, as calculated by Formula 1.

[0128] [Formula 1]

[0129] Crystallinity (%) = [Ic / (Ic+Ia)] × 100

[0130] In Formula 1, Ic is the sum of the integrated values ​​of the scattering intensity of the crystalline peak in the X-ray diffraction analysis spectrum of the soft magnetic alloy particles, and Ia is the sum of the integrated values ​​of the scattering intensity of the amorphous halo in the X-ray diffraction analysis spectrum of the soft magnetic alloy particles.

[0131] Specifically, after obtaining the XRD pattern of the soft magnetic alloy particles in the cross-sectional sample of the body 110, the crystallinity of the soft magnetic alloy particles can be calculated by Formula 1. The XRD pattern of the soft magnetic alloy particles can be obtained by a sample obtained by crushing and sieving the cross-sectional sample of the body to a size greater than or equal to about 20 μm. The meaning of the term "about" and the like may include process errors, measurement errors, and the like that occur during the manufacturing process that can be identified by a person of ordinary skill in the art. For example, "about X" (where "X" is a number) may mean exactly "X", or may include a tolerable deviation from "X" that can be identified by a person of ordinary skill in the art due to process errors, measurement errors, and the like that occur during the manufacturing process.

[0132] An average crystal size of nanocrystals included in the soft magnetic alloy particles may be less than or equal to about 20 nm, for example, less than or equal to about 18 nm.

[0133] For example, the average crystal size of the nanocrystals can be calculated using the full width at half maximum (FWHM) of the major peak in the XRD pattern using the Scherer equation.

[0134] Specifically, after obtaining the XRD pattern of the soft magnetic alloy particles in the cross-sectional sample of the body 110, the average crystal size of the nanocrystals can be calculated by using the full width at half maximum. The XRD pattern of the soft magnetic alloy particles can be obtained by a sample obtained by crushing and sieving the cross-sectional sample of the body to a size greater than or equal to about 20 μm.

[0135] For example, the average crystal size of the nanocrystals can also be measured in a scanning electron microscope (SEM) image or a transmission electron microscope (TEM) image of a cross-sectional sample of the main body, in a soft magnetic alloy particle corresponding to a coarse powder magnetic particle having a particle size of about 10 μm to about 30 μm. Specifically, in the image of the cross-sectional sample, with the center point in the L-axis direction as a reference, the average crystal size of the nanocrystals can be obtained by measuring the size of the nanocrystals produced inside the coarse powder magnetic particles observed in a plurality of regions (e.g., 10 regions) at predetermined intervals in the T-axis direction and calculating the average value. The intervals between the plurality of regions can be adjusted according to the ratio of the scanning electron microscope (SEM) image or the transmission electron microscope (TEM) image, and can be equally spaced. At this time, all of the plurality of regions must be located in the main body, and if all of the 10 points are not located in the main body, the position of the reference point can be changed or the intervals between the 10 points can be adjusted.

[0136] Since the soft magnetic alloy particles are the same as the above-mentioned soft magnetic alloy particles, the remaining description is omitted.

[0137] In an embodiment, an insulating film (not shown) may be additionally provided on the surface of the soft magnetic alloy particles to impart insulating properties and ensure inductance.

[0138] The insulating film may be provided in one or more layers, or may be provided in up to three layers. For example, the insulating film may be an organic film including epoxy resin, polyimide resin, liquid crystal polymer, or a combination thereof, may be an inorganic film including silicon monoxide (SiO) or silicon dioxide (SiO2), or may be a metal oxide film including aluminum oxide (Al2O3), iron oxide (Fe2O3, FeO), or chromium oxide (CrO). When the insulating film is a metal oxide film, the metal oxide film may include a metal element contained in the soft magnetic alloy particles, but is not limited thereto.

[0139] The thickness of the insulating film may be about 1% to about 20% of the particle diameter of the soft magnetic alloy particles.

[0140] If the thickness of the insulating film exceeds about 20% of the particle diameter of the soft magnetic alloy particles, the magnetic permeability and magnetic susceptibility may decrease, so it is desirable to make the thickness as thin as possible.

[0141] The coil 130 is disposed inside the body 110 and plays a role of exhibiting inductor characteristics. For example, when the inductor 100 is used as a power inductor, the coil stores an electric field as a magnetic field to maintain an output voltage, thereby stabilizing the power supply of the electronic device. The coil may be any type of a winding type formed by a winding method, a thin film type formed by a thin film method, and a multilayer type formed by a stacking method, but hereinafter, a thin film type coil may be described as an example.

[0142] The coil 130 may include an upper coil 131 and a lower coil 132 respectively disposed on the upper and lower surfaces of the support member 120. The upper coil 131 and the lower coil 132 may be coil layers disposed opposite to each other with respect to the support member 120.

[0143] The upper coil 131 and the lower coil 132 may be formed as a plated layer on the support member 120 through a plating process or a photolithography method.

[0144] The coil 130 can be made of a material with excellent conductivity, for example, at least one metal selected from gold (Au), silver (Ag), platinum (Pt), copper (Cu), nickel (Ni), palladium (Pd), aluminum (Al), titanium (Ti), etc. or their alloys, but is not limited to this, and any conventional conductive material can be used without particular limitation.

[0145] The support member 120 may be made of any material capable of supporting the upper coil 131 and the lower coil 132 without particular limitation, for example, a copper clad laminate (CCL), a polypropylene glycol (PPG) substrate, a ferrite substrate, a metal-based soft magnetic substrate, etc. In addition, an insulating substrate made of an insulating resin may be used. The insulating resin may include a thermosetting resin such as an epoxy resin, a thermoplastic resin such as a polyimide, or a resin in which a reinforcing material such as glass fiber or an inorganic filler is impregnated in a thermosetting resin or a thermoplastic resin (such as a prepreg, ajinomoto build-up film (ABF, ajinomoto build-up film), FR-4, bismaleimide triazine (BT) resin, a photoimageable dielectric (PID) resin, etc.). In terms of maintaining rigidity, an insulating substrate including glass fiber and epoxy resin may be used, but is not limited thereto.

[0146] The upper and lower surfaces of the support member 120 may be penetrated to form a hole, and the hole may be filled with a magnetic material to form the core 150. The core filled with the magnetic material may improve inductance.

[0147] The upper coil 131 and the lower coil 132 stacked on both surfaces of the support member are electrically connected through a via hole 140 penetrating the support member 120 .

[0148] The via hole 140 may be formed by forming a through hole using a mechanical drill or a laser drill and filling the through hole with a conductive material through plating.

[0149] The via 140 may not be particularly limited in shape or material as long as it electrically connects both the upper coil 131 and the lower coil 132 respectively disposed on the upper and lower surfaces of the support member 120. Here, the upper and lower surfaces are determined based on the stacking direction of the coil patterns in the drawing.

[0150] The via 140 may include a conductive material such as copper (Cu), aluminum (Al), silver (Ag), tin (Sn), gold (Au), nickel (Ni), lead (Pd), or alloys thereof.

[0151] The upper coil 131 and the lower coil 132 may be covered with an insulating layer 133 so that they do not directly contact the magnetic material included in the body 110 .

[0152] The insulating layer 133 may serve to protect the upper coil 131 and the lower coil 132 .

[0153] The insulating layer 133 may be formed using any material including insulating materials, for example, insulating materials used for conventional insulating coatings, such as epoxy resins, polyimide resins, liquid crystal polymer resins, etc., wherein known photoimageable dielectric (PID) resins may be used, but are not limited thereto.

[0154] The insulating layer 133 may be formed by a vapor deposition method or the like, but is not limited thereto, and is formed to be stacked on both surfaces of the support member.

[0155] The inductor 100 according to the embodiment further includes external electrodes 161 and 162 disposed on an outer surface of the body 110 and electrically connected to the upper coil 131 and the lower coil 132 , respectively.

[0156] The external electrodes 161 and 162 are electrically connected to lead-out terminals of the upper coil 131 and the lower coil 132 , respectively exposed at both sides of the body 110 .

[0157] When the inductor 100 is mounted on an electronic device, the external electrodes 161 and 162 are used to electrically connect the coil 130 inside the inductor to the electronic device.

[0158] The external electrodes 161 and 162 may include a conductive paste layer formed using a conductive paste including a conductive metal, and the conductive metal may be at least one of copper (Cu), nickel (Ni), tin (Sn), and silver (Ag), or an alloy thereof.

[0159] The external electrodes 161 and 162 may include a plated layer formed on the conductive paste layer.

[0160] The plating layer may include at least one selected from nickel (Ni), copper (Cu), and tin (Sn), and, for example, a nickel (Ni) layer and a tin (Sn) layer may be sequentially formed.

[0161] Hereinafter, the wound type inductor 200 and the multilayer type inductor 300 will be described in detail. Hereinafter, the wound type inductor 200 and the multilayer type inductor 300 will be described only with respect to the configuration difference from the film type inductor 100. The description of the film type inductor 100 is applicable to the remaining configurations of the wound type inductor 200 and the multilayer type inductor 300.

[0162] Figure 8 A perspective view of a wound inductor according to another embodiment is schematically shown, and Fig. 9 Schematically shows Figure 8 Taken along line Ⅱ-Ⅱ' Figure 8 The cross section of the inductor.

[0163] The wound inductor 200 according to the embodiment includes a body 210 including a magnetic material including soft magnetic alloy particles, a coil 230 located inside the body, and external electrodes 261 and 262 located on an outer surface of the body 210 .

[0164] In the embodiment, the body 210 includes a molded part 211, a cover part 212 disposed on one surface of the molded part 211, and a core 250 protruding from one surface of the molded part 211. The coil 230 is disposed between one surface of the molded part 211 and the cover part 212, and the core 250 penetrates the coil 230.

[0165] The body 210 of the wound inductor 200 includes a molded part 211 and a cover part 212 disposed on one surface of the molded part 211, and further includes a core 250 disposed to protrude from one surface of the molded part 211. Here, the coil 230 may be disposed on one surface of the molded part 211 to wind around the core 250.

[0166] The body 210 includes a magnetic material, and the magnetic material includes soft magnetic alloy particles according to an embodiment. In other words, at least one of the forming part 211, the cover part 212 and the core 250 includes a magnetic material containing soft magnetic alloy particles. For example, the forming part 211 can be formed by filling the magnetic material in a mold. As another example, the forming part 211 can be formed by filling a composite material including a magnetic material and a resin in the mold. A process of applying high temperature and high pressure to the magnetic material or composite material in the mold may be performed in addition, but is not limited thereto. The forming part 211 and the core 250 can be formed integrally by the above-mentioned mold without a boundary therebetween. The cover part 212 can be formed by dispersing a magnetic composite sheet in a resin with a magnetic material on the forming part 211 and the coil 230, and then heating and pressing it.

[0167] In the wound type inductor 200 , a lead portion (not shown) penetrates the molded part 211 to be connected to the external electrodes 261 and 262 .

[0168] The description of the magnetic material and the soft magnetic alloy particles in the thin film type inductor 100 according to the embodiment may be equally applied to the magnetic material and the soft magnetic alloy particles in the body 210 .

[0169] In the wound inductor 200, the surface of the coil 230 may be covered with an insulating layer 231, and the insulating layer 231 serves to insulate the magnetic material of the body 210 from the coil 230. In addition, the description of the insulating layer 133 may be applied to the insulating layer 231 as well.

[0170] The wound inductor 200 is different from the film-type inductor 100 in the configuration of the coil 230 and the presence or absence of a support member.

[0171] In the wound inductor 200, the coil 230 is a wound type and does not include a support member. The coil 230 may be a wound coil formed by winding a metal wire (such as a copper wire (Cu-wire)) whose surface is covered with an insulating layer 231, etc. The metal wire may be a flat wire, but is not limited thereto.

[0172] exist Figure 8 , the coil 230 is shown as an alpha (α) shaped wound wire, but this is exemplary only and may be an edge wound wire.

[0173] Fig.10 A perspective view schematically shows a multilayer inductor according to another embodiment, and Fig.11 Schematically shows Fig.10 Taken along line III-III' Fig.10 Cross-sectional view of the inductor shown in .

[0174] The multilayer type inductor 300 according to the embodiment includes a body 310 including a magnetic material including soft magnetic alloy particles, a coil 330 located in the body, and external electrodes 361 and 362 located on an outer surface of the body 310. The body 310 includes a plurality of magnetic sheets including a magnetic material.

[0175] The description of the thin film type inductor 100 according to the embodiment may be equally applied to the magnetic material and the soft magnetic alloy particles in the body 310 .

[0176] For example, the body 310 is obtained by stacking a plurality of magnetic sheets including magnetic materials in the thickness direction and firing them, wherein the shape and size of the body 310 and the number of stacked magnetic sheets are not limited to the shape and size of the body and the number of stacked magnetic sheets shown in the embodiment.

[0177] On one surface of the plurality of magnetic sheets, a conductor pattern for forming the coil 330 is formed, and a conductive via may be formed to electrically connect the upper conductive pattern and the lower conductive pattern in the thickness direction of the magnetic sheet. That is, the coil 330 includes a plurality of conductor patterns formed in the plurality of magnetic sheets and a plurality of conductive vias that electrically connect the plurality of conductor patterns.

[0178] Therefore, one ends of the conductor patterns formed on each magnetic sheet are electrically connected to each other through the conductive vias formed on the adjacent magnetic sheets, thereby forming the coil 330 .

[0179] The surface of the coil 330 may be covered with an insulating layer 331, and the insulating layer 331 may play a function of insulating the magnetic material of the body 310 from the coil 330. The insulating layer 331 may be applied in the same manner as described above for the insulating layer 133.

[0180] Both ends of the coil 330 may be led out through the body 310 to respectively contact and be electrically connected to a pair of external electrodes 361 and 362 formed on the body 310 .

[0181] In particular, both ends of the coil 330 may be led out through both ends of the body 310 , and a pair of external electrodes 361 and 362 may be formed at both ends of the body 310 from which the coil 330 is led out.

[0182] The conductor pattern may be formed by thick-film printing a conductive paste for forming the conductor pattern on a green sheet for forming the magnetic sheet, or by coating, depositing or sputtering the conductive paste, but is not limited thereto.

[0183] The conductive vias may be formed by forming through holes in each sheet in the thickness direction and then filling the through holes with a conductive paste or the like, but are not limited thereto.

[0184] In addition, the conductive metal included in the conductive paste for forming the conductor pattern may be one selected from silver (Ag), palladium (Pd), platinum (Pt), nickel (Ni) and copper (Cu) or an alloy thereof, but the present invention is not limited thereto.

[0185] The soft magnetic alloy particles, when included in the body of the above-mentioned thin film type, wound type or multilayer type inductor, can maintain high magnetic saturation characteristics and improve electromagnetic performance due to their excellent characteristics.

[0186] In addition to the above-mentioned inductors, the soft magnetic alloy particles can also be used in magnetic products such as transformers, motors or stators of motors.

[0187] Hereinafter, specific examples of the present invention are given. However, the examples described below are only intended to specifically illustrate or explain the present invention, and the scope of the present invention should not be limited thereto.

[0188] [Example]

[0189] (Preparation Example 1: Preparation of Soft Magnetic Alloy Particles)

[0190] Fe, Co, Ge, B, P and Cu raw materials were prepared, and the prepared raw materials were weighed to have the composition formula shown in Table 1. The weighed raw materials were mixed, and a master alloy was prepared using an arc melting method. After the prepared master alloy was melted, it was rapidly cooled in a rapid cooling device to prepare a soft magnetic initial alloy.

[0191] The soft magnetic alloy particles of Examples 1 to 5 and Comparative Examples 1 to 11 represented by the composition formulas in Table 1 were prepared by heat treating the initial soft magnetic alloy to the heat treatment temperature (° C.) shown in Table 1.

[0192] [Table 1]

[0193]

[0194] (Preparation Example 2: Production of Inductor)

[0195] A body including a magnetic material in which soft magnetic alloy particles prepared according to Preparation Example 1 were dispersed in a resin was manufactured, and then an inductor including the body was manufactured.

[0196] [Experimental example]

[0197] (Experimental Example 1: Analysis of Ge content difference between amorphous phase and crystalline phase)

[0198] The Ge content in the amorphous phase and the crystalline phase of the soft magnetic alloy particles included in each of the inductors according to the example and the comparative example and the difference in the Ge content were analyzed.

[0199] After the inductor was placed in an epoxy resin mixed solution and then cured, the L-axis and T-axis direction surfaces of each inductor were polished to a 1 / 2 point in the W-axis direction and fixed in a vacuum atmosphere chamber, thereby obtaining a cross-sectional sample of the body.

[0200] With respect to the cross-sectional sample of the obtained body, line analysis of the soft magnetic alloy particles dispersed in the resin was performed by using EDS (Energy Dispersive X-ray Spectrometer) installed in a transmission electron microscope (TEM).

[0201] Specifically, in the online analysis, the online analysis is obtained by point quantitative analysis based on the inner 20nm and outer 200nm of the surface of any nanocrystalline particle, and the maximum value of the content of the Ge element inside the nanocrystalline particle and the maximum value of the content of the Ge element in the amorphous phase part of the nanocrystalline particle are compared. The point quantitative analysis is performed at 6 points respectively, and the average value of the Ge content is calculated.

[0202] Herein, each average Ge atomic content (Ge(a), Ge(c)) (unit: at%) and the content difference (Ge(a)-Ge(c)) (unit: at%) in the amorphous phase and the crystalline phase are shown in Table 2.

[0203] Referring to Table 2, the average Ge atomic content in the amorphous phase (Ge (a)) is higher than the average Ge atomic content in the crystalline phase (Ge (c)). Therefore, the Ge element with a relatively large atomic weight (compared with the atomic weight of Si element, etc.) can be retained in the amorphous phase and play a role in suppressing the growth of nanocrystals in the soft magnetic alloy particles.

[0204] [Table 2]

[0205]

[0206] (Experimental Example 2: DTA analysis)

[0207] By using a rapid cooling strip device, the soft magnetic alloy particles of the examples and comparative examples were prepared into a strip shape with a thickness of 20 μm for DTA analysis. Through this analysis, the first crystallization temperature T of the particles was examined. x1 and the second crystallization temperature T x2 , and the results are shown in Table 1.

[0208] Referring to Table 1, in Examples 1 to 5, as the second crystallization temperature T x2 Increase, due to the first crystallization temperature T x1 and the second crystallization temperature T x2 The difference between them exceeds 100°C, so the thermal treatment process window for forming nanocrystals is improved.

[0209] (Experimental Example 3: Analysis of Crystal Size and Crystal Fraction)

[0210] First, XRD patterns of soft magnetic alloy particles in cross-sectional samples of the bodies according to Examples and Comparative Examples were obtained.

[0211] The average nanocrystal size of each soft magnetic alloy particle was measured by using the full width at half maximum (FWHM) of the main peak of the XRD pattern and the Scherer formula represented by Formula 2. The results are shown in Table 1.

[0212] [Formula 2]

[0213]

[0214] In Formula 2, D is the average crystal size, λ is the wavelength of the XRD target, β is the full width at half maximum (FWHM), and θ is half of the peak 2θ of the XRD pattern.

[0215] Referring to Table 1, the nanocrystals of Examples 1 to 5 have an average crystal size of less than or equal to 20 nm (about 17 nm). In contrast, the nanocrystals of Comparative Examples 1 to 11 have an average crystal size of greater than or equal to about 20 nm.

[0216] Furthermore, after XRD analysis, the crystal fraction was obtained by fitting the data and calculating the ratio of the amorphous area to the crystalline area according to [Formula 1].

[0217] Referring to Table 1, Examples 1 to 5 showed improved crystal fractions of 59% or more. In contrast, Comparative Examples 1 to 11 showed crystal fractions of less than 59%.

[0218] (Experimental Example 4: Evaluation of Electromagnetic Performance)

[0219] The magnetic permeability at a frequency of 1 kHz and the iron loss at a magnetic field of 0.2 T and 100 kHz were measured, and the results are shown in Table 1.

[0220] Referring to Table 1, Examples 1 to 5 exhibited a magnetic permeability of 5300 or more and an iron loss of 1590 mW / cc or less, which confirmed excellent electromagnetic performance. In contrast, Comparative Examples 1 to 11 exhibited a magnetic permeability of less than 5300 and an iron loss of more than 1590 mW / cc, which confirmed deteriorated electromagnetic performance.

[0221] Furthermore, referring to Table 1, compared with Comparative Examples 1 to 11, Examples 1 to 5 simultaneously exhibited the above-described effects and similar levels of Ms values.

[0222] While the present invention has been described in connection with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

Claims

1. A soft magnetic alloy particle, comprising: nanocrystals and an amorphous phase, as well as Fe and Ge, wherein the average content of Ge in the amorphous phase based on atomic percentage is Ge(a), the average content of Ge in the nanocrystals based on atomic percentage is Ge(c), and Ge(a) - Ge(c) > 0.

2. The soft magnetic alloy particle according to claim 1, wherein the composition of the soft magnetic alloy particle is represented by Composition Formula 1: Composition Formula 1 Feb a Co b Ge c M d wherein, in Composition Formula 1, a, b, c, and d respectively represent the atomic percentage contents of the corresponding elements, 0 < a ≤ 90, 0 ≤ b ≤ 10, 0 < c ≤ 5, 0 < d ≤ 20, a + b + c + d = 100, and M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S, or a combination thereof.

3. The soft magnetic alloy particle according to claim 2, wherein M does not include Si.

4. The soft magnetic alloy particle according to claim 2, wherein c satisfies 0.5 ≤ c ≤ 4.

5. The soft magnetic alloy particle according to claim 2, wherein a satisfies 70 ≤ a ≤ 80.

6. The soft magnetic alloy particle according to claim 2, wherein b satisfies 2 ≤ b ≤ 6.

7. The soft magnetic alloy particle according to claim 2, wherein a and b satisfy 75 ≤ a + b ≤ 90.

8. The soft magnetic alloy particle according to claim 2, wherein d satisfies 10 ≤ d ≤ 20.

9. The soft magnetic alloy particle according to claim 2, wherein Ge(a) and Ge(c) satisfy 0.1 ≤ Ge(a) - Ge(c) ≤ 0.

7.

10. The soft magnetic alloy particle according to claim 2, wherein M includes B, P, Cu, or a combination thereof.

11. The soft magnetic alloy particle according to claim 1, wherein the crystallinity of the soft magnetic alloy particle is greater than or equal to 59% and less than or equal to 70%.

12. The soft magnetic alloy particle according to claim 1, wherein the average crystal size of the nanocrystals is less than or equal to 20 nm.

13. An inductor, comprising: a body including a magnetic material, the magnetic material including soft magnetic alloy particles; a coil located in the body; and an external electrode located on the outer surface of the body, wherein the soft magnetic alloy particles include nanocrystals and an amorphous phase, and include Fe and Ge, and the average content of Ge in the amorphous phase based on atomic percentage is Ge(a), and the average content of Ge in the nanocrystals based on atomic percentage is Ge(c), and Ge(a) - Ge(c) > 0.

14. The inductor according to claim 13, wherein the composition of the soft magnetic alloy particle is represented by Composition Formula 1: Composition Formula 1 Feb a Co b Ge c M d wherein, in Composition Formula 1, a, b, c, and d respectively represent the atomic percentage contents of the corresponding elements, 0 < a ≤ 90, 0 ≤ b ≤ 10, 0 < c ≤ 5, 0 < d ≤ 20, a + b + c + d = 100, and M includes B, P, Cu, Nb, Cr, C, Ni, Al, Mn, Ag, Zn, Sn, As, Sb, Bi, N, O, S or a combination thereof.

15. The inductor according to claim 14, wherein M does not include Si.

16. The inductor according to claim 14, wherein c satisfies 0.5≤c≤4.

17. The inductor according to claim 13, wherein: The soft magnetic alloy particles have a crystallinity greater than or equal to 59% and less than or equal to 70%.

18. The inductor according to claim 13, wherein: The average crystal size of the nanocrystals is less than or equal to 20 nm.

19. The inductor according to claim 13, wherein: The coil includes a support member and an upper coil and a lower coil respectively located on an upper surface and a lower surface of the support member, and The upper coil and the lower coil are connected through a via hole penetrating the support member.

20. The inductor according to claim 13, wherein The body includes a molded portion, a cover portion on one surface of the molded portion, and a core protruding from one surface of the molded portion, The coil is located between one surface of the molded portion and the cover portion, and the core penetrates the coil so that the coil is wound around the core.

21. The inductor according to claim 13, wherein The body includes a plurality of magnetic sheets including the magnetic material.

22. The inductor according to claim 21, wherein The coil includes a plurality of conductor patterns formed in the plurality of magnetic sheets and a plurality of conductive vias penetrating the respective magnetic sheets in a thickness direction of the magnetic sheets to electrically connect adjacent conductor patterns.

Citation Information

Cited By

  • Iron-based magnetically soft alloy strip and preparation method and application thereof

    CN120319561A