Injectable hydrogel material as well as preparation method and application thereof
Through the combination of modified natural polysaccharides and compound metal salt solutions, an injectable hydrogel is formed, which solves the problems of difficult submucosal injection and insufficient gel-forming strength in ESD, and achieves rapid gel-formation, high strength and biodegradability. Suitable for ESD surgery, improving surgical safety and operating field of view.
Patent Information
- Application Number
- CN202411012740.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-22
AI Technical Summary
Existing hydrogel materials for submucosal injection in ESD have problems such as difficulty in injection, difficulty in degradation, and insufficient gel-forming strength, making it difficult to meet surgical needs.
It uses a combination of modified natural polysaccharide solution and compound metal salt solution to form an injectable hydrogel through physical cross-linking. It has rapid gel formation, high strength, high transparency and biodegradability, and is suitable for the requirements of different surgical sites.
It achieves rapid gel formation in situ of the lesion, improves surgical safety and operating field of view, and reduces the risk of perforation and bleeding. The gel naturally degrades in the body without the need for eluents, and has good biocompatibility and low cost.
Smart Images

Figure CN118807002A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of medical materials, and more particularly to an injectable hydrogel material and a preparation method and application thereof. Background Art
[0002] Endoscopic submucosal dissection (ESD) is one of the minimally invasive treatments for early gastrointestinal cancer and precancerous lesions in recent years. It has the advantages of less trauma, less pain, and faster recovery. It can greatly reduce the harm and pain caused by surgery to patients. It is suitable for the resection of submucosal benign tumors, early mucosal cancer, and lesions with a tendency to cancer in the esophagus, stomach, duodenum, and upper gastrointestinal tract, colon, and rectum. The standard steps of the ESD procedure usually include: circumferential marking to determine the boundary of the lesion, submucosal injection at different locations around the lesion, circumferential cleaning, submucosal dissection, and wound treatment. Among them, intraoperative submucosal injection to elevate the lesion is the key to safety and success, because it can elevate the mucosa to be removed and isolate it from the muscle layer, which can reduce the risk of perforation and bleeding when performing an overall resection.
[0003] A variety of submucosal injection materials (SIMs) have been used in ESD, including normal saline, hypertonic saline, glucose solution, glycerol, hydroxypropyl methylcellulose, and sodium hyaluronate. However, these products have many defects and are difficult to meet the treatment requirements. Although normal saline has the characteristics of strong biocompatibility, low cost, and low toxicity, its strong fluidity leads to weak support for the mucosa. During the operation, it will penetrate into the surrounding tissues, making it difficult to maintain the height of the submucosal pad for a long time, and repeated injections are required. Viscous polymer solutions have better effects than normal saline in maintaining the elevation time, such as sodium hyaluronate, sodium carboxymethyl starch, and fibrin glue, but more and more ESD clinical cases have shown that with the increase of operation time, a series of intraoperative and postoperative problems such as perforation and delayed bleeding caused by fluid leakage and mucosal collapse are still difficult to solve.
[0004] Hydrogel is a polymer with a three-dimensional network structure, which has good permeability, transparency, biocompatibility and biodegradability, and is widely used in the biomedical field. During ESD surgery, the hydrogel precursor is injected under the mucosa in the form of a liquid, and then gels in situ under physiological conditions such as temperature, pH value, enzyme and exogenous light-induced polymerization to form a solid-like hydrogel. The gel can be used as a mucosal pad to separate the mucosal layer from the muscle layer, reduce surgical complications such as bleeding and perforation during surgery, and avoid repeated injections during surgery. For example, a patent application with publication number CN116510092A discloses a thermosensitive hydrogel that is injected into the submucosal layer in the form of a sol at room temperature, and then spontaneously gels in situ at body temperature and lifts the mucosa, which can significantly shorten the operation time. However, when it is clinically used in ESD surgery, once the body temperature is reached in the long injection tube, the thermosensitive hydrogel may gel prematurely, causing the long tube to be blocked, making injection difficult. The patent with publication number CN116688253A mentions an acrylamide-based hydrogel. Although the gelling speed of the gel is fast, the residual hydrogel cannot be degraded and needs to be eluted. In addition, shear-thinning hydrogels are also being studied for submucosal injection materials, but pure physical cross-linked hydrogels generally have poor strength and are not in line with clinical requirements. Therefore, the development of a new in situ curing hydrogel for ESD mucosal injection is a new trend in current ESD research.
[0005] How to develop an injectable hydrogel material and its preparation method and its application in the preparation of materials for separating the mucosal layer and the muscle layer in endoscopic submucosal dissection to address the shortcomings of existing submucosal injection hydrogels in ESD, such as difficulty in injection, difficulty in degradation, and insufficient gel strength, is an urgent problem that technicians in this field need to solve. Summary of the invention
[0006] In view of this, the present invention provides an injectable hydrogel material and a preparation method and application thereof.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] An injectable hydrogel material comprises a modified natural polysaccharide solution and a compound metal salt solution, wherein the volume ratio of the modified natural polysaccharide solution to the compound metal salt solution is (1-3):(1-3).
[0009] Beneficial effects of the present invention:
[0010] The injectable hydrogel material of the present invention mixes a modified natural polysaccharide solution and a metal ion salt solution, and quickly forms a gel through physical cross-linking. It has the advantages of easy availability of raw materials, low cost, simple injection, rapid gelation in situ of the lesion, high strength after gelation, high transparency and biodegradability. In addition, it can also improve the intraoperative hemostatic effect, overcome the shortcomings of existing hydrogel materials such as easy clogging during injection, harsh gelation conditions, poor gel strength and the need for elution, and can also achieve multiple clinical functions such as protecting the mucosa, reducing perforation or bleeding, and improving surgical visibility.
[0011] 1) The present invention has excellent effects. After the modified natural polysaccharide solution and the compound metal salt solution are mixed, no mechanical stirring is required. A jelly-like gel can be formed within 20-120 seconds upon contact, and the reaction is rapid;
[0012] 2) The modulus of the hydrogel can be changed by changing the concentration of the modified natural polysaccharide solution and the compound metal salt solution, so that the gel can be adapted to the requirements of different surgical sites;
[0013] 3) The gel shape remains persistent, lifting the mucosal layer of the lesion area and effectively separating it from the muscularis propria, which is conducive to the complete removal of the lesion and avoids unnecessary risks caused by cutting through the digestive tract during the removal process;
[0014] 4) The gel has good transparency, which improves the doctor's operating field of vision;
[0015] 5) The hydrogel material of the present invention has good biodegradability, does not require the use of eluents, and can be naturally degraded in the body;
[0016] 6) The raw materials used in the present invention are low in cost and have good biocompatibility, and are safe and reliable to the human body.
[0017] 7) In addition to having a low injection pressure, the hydrogel of the present invention has a significant effect of lifting the mucosa, can effectively lift the lesion, and has the effect of hemostasis and antibacterial, promoting postoperative wound healing.
[0018] Furthermore, the modified natural polysaccharide solution is a solution of one or more of carboxymethyl chitosan, sodium alginate, oxidized hyaluronic acid or modified starch;
[0019] The composite metal salt solution comprises a metal salt solution, an additive and a hemostatic agent, wherein the metal ion in the metal salt solution is Ca 2+ , Ba 2+ 、Zn 2+ or Fe 2+ One or more of the .
[0020] The beneficial effects of adopting the above further technical solution are as follows: the modified natural polysaccharide has good biocompatibility and degradability, and the groups on the molecular chain can quickly react with metal ions to form a gel by forming physical crosslinks.
[0021] Furthermore, the acid ions in the above metal salt solution are Cl - 、SO4 2- PO4 3- or CO3 2- One or more of the .
[0022] Furthermore, the concentration of the modified natural polysaccharide in the modified natural polysaccharide solution is 0.05%-1.0% (w / v), and the concentration of the metal salt in the composite metal salt solution is 0.02%-0.4% (w / v).
[0023] Furthermore, the solvent in the modified natural polysaccharide solution or the composite metal salt solution is one or more of pure water, sodium chloride solution and phosphate buffer solution.
[0024] Furthermore, the sodium chloride solution is a sodium chloride aqueous solution with a concentration of 0.9% (w / v), and the phosphate buffer is a sodium dihydrogen phosphate or potassium dihydrogen phosphate buffer with a concentration of 10% (w / v), and the pH value is 5.
[0025] Furthermore, the concentration of the additive is 0.01%-0.02% (w / v), and the concentration of the hemostatic agent is 0.01%-0.02% (w / v).
[0026] The beneficial effect of adopting the above further technical solution is that it can improve the hemostasis effect during surgery.
[0027] Furthermore, the above-mentioned additive is one or more of sodium indigo disulfonate, methylene blue, brilliant blue, trypan blue or toluidine blue, and the above-mentioned hemostatic agent is one or more of vancomycin hydrochloride, ε-polylysine, halloysite, montmorillonite or curcumin.
[0028] The beneficial effect of adopting the above further technical solution is: improving the visibility of the gel during surgery.
[0029] Furthermore, the volume ratio of the modified natural polysaccharide solution to the composite metal salt solution is 1:1, 2:1 or 3:1.
[0030] The present invention also provides a method for preparing an injectable hydrogel material, comprising the following steps:
[0031] The modified natural polysaccharide solution and the compound metal salt solution are respectively injected at the same position so that the modified natural polysaccharide solution and the compound metal salt solution are contacted to form gel, thereby obtaining the above-mentioned injectable hydrogel material.
[0032] Furthermore, the time required for the above contact gelation is 20 to 120 seconds.
[0033] Furthermore, the above injection is performed using a syringe dedicated to endoscopes.
[0034] Furthermore, the preparation method of the modified natural polysaccharide solution comprises the following steps:
[0035] One or more of carboxymethyl chitosan, sodium alginate, oxidized hyaluronic acid or modified starch is added into a solvent and mixed evenly to obtain a modified natural polysaccharide solution.
[0036] Furthermore, the preparation method of the composite metal salt solution comprises the following steps:
[0037] Ca 2+ , Ba 2+ 、Zn 2+ or Fe 2+ One or more of the salts are added to a solvent to dissolve, and additives and hemostatic agents are added and mixed evenly to obtain a composite metal salt solution.
[0038] The present invention also provides an application of the injectable hydrogel material or the preparation method in preparing a material for separating a mucosal layer and a muscle layer in endoscopic submucosal dissection. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a diagram showing the process of mixing the modified natural polysaccharide solution and the compound metal salt solution to form a hydrogel in Example 1;
[0040] Figure 2 This is a demonstration diagram of cutting hydrogel with an electric knife in Example 1;
[0041] Figure 3 This is a scanning electron microscope image of the hydrogel in Example 1;
[0042] Figure 4 The storage modulus and loss modulus of the hydrogel in Examples 1-5 vary with strain;
[0043] Figure 5 is a curve showing the storage modulus and loss modulus of the hydrogel in Comparative Example 1-2 as a function of frequency;
[0044] Figure 6 The degradation of the hydrogels of Examples 1 and 3 after being immersed in PBS solution for 11 days. DETAILED DESCRIPTION
[0045] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] Example 1
[0047] The method for preparing an injectable hydrogel material comprises the following steps:
[0048] (1) Preparation of modified natural polysaccharide solution:
[0049] Carboxymethyl chitosan and sodium alginate were added into solvent pure water at a mass ratio of 1:1 and mixed evenly to obtain a modified natural polysaccharide solution with a total concentration of 0.05% (w / v) of the modified natural polysaccharide.
[0050] (2) Preparation of composite metal salt solution:
[0051] FeCl2 is dissolved in pure water, and the additive methylene blue and the hemostatic agent vancomycin hydrochloride are added and mixed evenly to obtain a complex metal salt solution with a metal salt concentration of 0.02% (w / v), an additive concentration of 0.01% (w / v), and a hemostatic concentration of 0.01% (w / v).
[0052] (3) The modified natural polysaccharide solution and the compound metal salt solution were injected into the same position using an endoscope-specific syringe in a volume ratio of 1:1, so that the modified natural polysaccharide solution and the compound metal salt solution were in contact for about 2 minutes to form a gel, thereby obtaining an injectable hydrogel material with a modulus of 45±2Pa.
[0053] Example 2
[0054] The method for preparing an injectable hydrogel material comprises the following steps:
[0055] (1) Preparation of modified natural polysaccharide solution:
[0056] Carboxymethyl chitosan and sodium alginate were added into solvent pure water at a mass ratio of 1:1 and mixed evenly to obtain a modified natural polysaccharide solution with a total concentration of 0.1% (w / v) of the modified natural polysaccharide.
[0057] (2) Preparation of composite metal salt solution:
[0058] CaSO4 is dissolved in pure water, and the additive methylene blue and the hemostatic agent vancomycin hydrochloride are added and mixed evenly to obtain a composite metal salt solution with a metal salt concentration of 0.04% (w / v), an additive concentration of 0.01% (w / v), and a hemostatic concentration of 0.01% (w / v).
[0059] (3) The modified natural polysaccharide solution and the compound metal salt solution were injected into the same position using a special endoscope syringe in a volume ratio of 1:1, so that the modified natural polysaccharide solution and the compound metal salt solution were in contact for about 1 minute to form a gel, thereby obtaining an injectable hydrogel material with a modulus of 50±2Pa.
[0060] Example 3
[0061] The method for preparing an injectable hydrogel material comprises the following steps:
[0062] (1) Preparation of modified natural polysaccharide solution:
[0063] Carboxymethyl chitosan and sodium alginate were added into a 0.9% NaCl aqueous solution at a mass ratio of 1:1 and mixed evenly to obtain a modified natural polysaccharide solution with a total concentration of 0.2% (w / v) of the modified natural polysaccharide.
[0064] (2) Preparation of composite metal salt solution:
[0065] CaSO4 is dissolved in pure water, and the additive methylene blue and the hemostatic agent vancomycin hydrochloride are added and mixed evenly to obtain a composite metal salt solution with a metal salt concentration of 0.06% (w / v), an additive concentration of 0.02% (w / v), and a hemostatic concentration of 0.02% (w / v).
[0066] (3) The modified natural polysaccharide solution and the compound metal salt solution were injected into the same position using an endoscope-specific syringe in a volume ratio of 2:1, so that the modified natural polysaccharide solution and the compound metal salt solution were in contact for about 50 seconds to form a gel, thereby obtaining an injectable hydrogel material with a modulus of 60±3Pa.
[0067] Example 4
[0068] The method for preparing an injectable hydrogel material comprises the following steps:
[0069] (1) Preparation of modified natural polysaccharide solution:
[0070] Sodium alginate and oxidized hyaluronic acid were added into solvent pure water at a mass ratio of 1:1 and mixed evenly to obtain a modified natural polysaccharide solution with a total concentration of 0.4% (w / v) of the modified natural polysaccharide.
[0071] (2) Preparation of composite metal salt solution:
[0072] CaSO4 is added to a 10% sodium dihydrogen phosphate solution (PH=5) to dissolve, and an additive methylene blue and a hemostatic agent vancomycin hydrochloride are added and mixed evenly to obtain a complex metal salt solution with a metal salt concentration of 0.08% (w / v), an additive concentration of 0.02% (w / v), and a hemostatic concentration of 0.02% (w / v).
[0073] (3) The modified natural polysaccharide solution and the compound metal salt solution were injected into the same position using an endoscope-specific syringe in a volume ratio of 2:1, so that the modified natural polysaccharide solution and the compound metal salt solution were in contact for about 40 seconds to form a gel, thereby obtaining an injectable hydrogel material with a modulus of 65±2Pa.
[0074] Example 5
[0075] The method for preparing an injectable hydrogel material comprises the following steps:
[0076] (1) Preparation of modified natural polysaccharide solution:
[0077] Carboxymethyl chitosan and sodium alginate were added into pure water at a mass ratio of 1:1 and dissolved to obtain a modified natural polysaccharide solution with a total concentration of 1.0% (w / v) of the modified natural polysaccharide.
[0078] (2) Preparation of composite metal salt solution:
[0079] CaSO4 is added to a 10% sodium dihydrogen phosphate solution (PH=5) and mixed evenly to dissolve, and an additive methylene blue and a hemostatic agent vancomycin hydrochloride are added and mixed evenly to obtain a composite metal salt solution with a metal salt concentration of 0.1% (w / v), an additive concentration of 0.02% (w / v), and a hemostatic concentration of 0.02% (w / v).
[0080] (3) The modified natural polysaccharide solution and the compound metal salt solution were injected into the same position using an endoscope-specific syringe in a volume ratio of 3:1, so that the modified natural polysaccharide solution and the compound metal salt solution were in contact for about 30 seconds to form a gel, thereby obtaining an injectable hydrogel material with a modulus of about 70±3Pa.
[0081] Comparative Example 1
[0082] The method for preparing an injectable hydrogel material comprises the following steps:
[0083] (1) Preparation of modified natural polysaccharide solution:
[0084] Carboxymethyl chitosan and sodium alginate were added to solvent pure water at a mass ratio of 1:1 and mixed evenly to obtain a modified natural polysaccharide solution with a total concentration of 2.0% (w / v) of the modified natural polysaccharide.
[0085] (2) Preparation of composite metal salt solution:
[0086] CaCl2 was dissolved in pure water, and the additive methylene blue and the hemostatic agent vancomycin hydrochloride were added and mixed evenly to obtain a composite metal salt solution with a metal salt concentration of 0.5% (w / v), an additive concentration of 0.01% (w / v), and a hemostatic concentration of 0.01% (w / v).
[0087] (3) The modified natural polysaccharide solution and the compound metal salt solution were injected into the same position using an endoscope-specific syringe in a volume ratio of 3:1, so that the modified natural polysaccharide solution and the compound metal salt solution were in contact for 25 seconds to form a gel, thereby obtaining an injectable hydrogel material. However, the modulus of the formed hydrogel was 35 kPa, which was relatively hard and brittle, and had poor mechanical properties.
[0088] Comparative Example 2
[0089] The method for preparing an injectable hydrogel material comprises the following steps:
[0090] (1) Preparation of modified natural polysaccharide solution:
[0091] Carboxymethyl chitosan and sodium alginate were added to solvent pure water at a mass ratio of 1:1 and mixed evenly to obtain a modified natural polysaccharide solution with a total concentration of 2.0% (w / v) of the modified natural polysaccharide.
[0092] (2) Preparation of composite metal salt solution:
[0093] CaCl2 was dissolved in pure water, and the additive methylene blue and the hemostatic agent vancomycin hydrochloride were added and mixed evenly to obtain a composite metal salt solution with a metal salt concentration of 0.7% (w / v), an additive concentration of 0.01% (w / v), and a hemostatic concentration of 0.01% (w / v).
[0094] (3) The modified natural polysaccharide solution and the compound metal salt solution were injected at the same position using an endoscope-specific syringe in a volume ratio of 3:1, so that the modified natural polysaccharide solution and the compound metal salt solution were in contact for 25 seconds to form a gel, thereby obtaining an injectable hydrogel material. The modulus of the hydrogel was 50 kPa. The gelation speed was too fast and the cross-linking density increased, which increased the injection pressure of liquid A and made the injection difficult.
[0095] In summary, the present invention has developed a gram-column hydrogel material with low injection pressure, fast gelation speed, adjustable mechanical properties, good transparency, good biocompatibility and degradability, and antibacterial and hemostatic effects on postoperative wounds. The material is very suitable as a submucosal pad material for ESD surgery and has very good clinical application scenarios.
[0096] like Figure 1 As shown, the process demonstration of Example 1 in which the modified natural polysaccharide solution and the compound metal salt solution are mixed to form a hydrogel;
[0097] like Figure 2 As shown, in the process of cutting the hydrogel with an electric knife in Example 1, the incision of the hydrogel is smooth;
[0098] like Figure 3 As shown, the scanning electron microscope image of the hydrogel after freeze drying in Example 1;
[0099] like Figure 4 As shown in the curves of the storage modulus and loss modulus of the hydrogel in Examples 1-5 as a function of strain, it can be seen that the hydrogel increases with the increase of the concentration of the polysaccharide solution and the concentration of the metal salt ion solution within a certain concentration range, and the maximum value reaches 70Pa.
[0100] like Figure 5 As shown, the curves of storage modulus and loss modulus of the hydrogel in Comparative Example 1-2 changing with frequency show that when the metal salt ion concentration is 0.5% and 0.7%, the gel modulus is too large, causing the gel to become brittle and unsuitable for clinical use.
[0101] like Figure 6 As shown, the degradation of the hydrogels of Example 1 and Example 3 after being immersed in PBS solution for 11 days, the degradation rate of the gel of Example 1 on the 11th day was about 35%, and the degradation rate of the gel of Example 3 was about 15%.
[0102] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An injectable hydrogel material, characterized in that: It comprises a modified natural polysaccharide solution and a compound metal salt solution, wherein the volume ratio of the modified natural polysaccharide solution to the compound metal salt solution is (1-3):(1-3).
2. The injectable hydrogel material according to claim 1, characterized in that: The modified natural polysaccharide solution is a solution of one or more of carboxymethyl chitosan, sodium alginate, oxidized hyaluronic acid or modified starch; The composite metal salt solution comprises a metal salt solution, an additive and a hemostatic agent. The metal ion in the metal salt solution is Ca 2+ , Ba 2+ 、Zn 2+ or Fe 2+ One or more of the .
3. The injectable hydrogel material according to claim 1, characterized in that: The concentration of the modified natural polysaccharide in the modified natural polysaccharide solution is 0.05%-1.0% (w / v), and the concentration of the metal salt in the compound metal salt solution is 0.02%-0.4% (w / v).
4. The injectable hydrogel material according to claim 1, characterized in that: The solvent in the modified natural polysaccharide solution or the composite metal salt solution is one or more of pure water, sodium chloride solution and phosphate buffer solution.
5. The injectable hydrogel material according to claim 1, characterized in that: The volume ratio of the modified natural polysaccharide solution to the composite metal salt solution is 1:1, 2:1 or 3:
1.
6. A method for preparing an injectable hydrogel material according to any one of claims 1 to 5, characterized in that: The following steps are involved: The modified natural polysaccharide solution and the compound metal salt solution are respectively injected at the same position so that the modified natural polysaccharide solution and the compound metal salt solution are contacted to form gel, thereby obtaining the injectable hydrogel material.
7. The method for preparing an injectable hydrogel material according to claim 6, characterized in that: The time required for the contact gelation is 20-120s.
8. The method for preparing an injectable hydrogel material according to claim 6, characterized in that: The preparation method of the modified natural polysaccharide solution comprises the following steps: One or more of carboxymethyl chitosan, sodium alginate, oxidized hyaluronic acid or modified starch is added into a solvent and mixed evenly to obtain a modified natural polysaccharide solution.
9. The method for preparing an injectable hydrogel material according to claim 6, characterized in that: The preparation method of the composite metal salt solution comprises the following steps: Ca 2+ , Ba 2+ 、Zn 2+ or Fe 2+ One or more of the salts are added to a solvent to dissolve, and additives and hemostatic agents are added and mixed evenly to obtain a composite metal salt solution.
10. Use of the injectable hydrogel material according to any one of claims 1 to 5 or the preparation method according to any one of claims 6 to 9 in preparing a material for separating a mucosal layer and a muscle layer in endoscopic submucosal dissection.