Alkane-olefin separation adsorbent as well as preparation method and application thereof
By using a molecular sieve adsorbent with a faujasite structure, combined with a specific preparation method, the problems of high energy consumption and difficulty in ensuring product purity during the separation of olefins and alkanes are solved, achieving efficient olefin adsorption and low catalytic activity, and improving separation efficiency and product purity.
Patent Information
- Application Number
- CN202310430705.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-22
AI Technical Summary
The existing technology has problems such as high energy consumption and difficulty in ensuring product purity during the separation process of olefins and alkanes. In particular, the activity of olefins causes adsorbent deactivation and isomerization reactions, which reduces separation efficiency and product purity.
A molecular sieve with a faujasite structure is used as an alkane-olefin separation adsorbent, and an adsorbent with high adsorption capacity and low catalytic activity is prepared through specific molding, heat treatment, binder crystallization, pH control and activation treatment methods. Used for adsorption separation of alkanes and alkenes.
It achieves highly selective adsorption and low catalytic activity of olefins, improves the separation efficiency of alkanes and olefins, reduces energy consumption, avoids isomerization reactions, and improves product purity.
Smart Images

Figure CN118807685A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an alkane-olefin separation adsorbent and a preparation method and application thereof. Background Art
[0002] Olefins are very important chemical raw materials, including ethylene and propylene, which have very large production and wide applications; butene, which has many types and different uses; and alpha olefins, which are used in different fields due to different carbon numbers. The main olefin resources are: ethylene / ethane resources, propylene / propane resources, C4 olefin resources containing butene, Fischer-Tropsch synthetic oil resources containing alpha olefins, and alkane dehydrogenation oil resources containing normal olefins and normal alkanes. In these olefin resources, olefins with the same or adjacent carbon numbers coexist with alkanes, so in order to obtain high-purity olefins, they must be separated.
[0003] The process of separating ethylene and propylene by low-temperature distillation in industry has high energy consumption, but the product purity is high and the technology is mature. 4 + The difference in boiling points between olefins and alkanes with the same carbon number is very small, and the difference in boiling points between olefin isomers is also very small, so distillation separation is very difficult and the energy consumption is very high. Distillation separation is even more unrealistic for the separation of a series of olefin and alkane mixtures with a wider carbon number.
[0004] Adsorption separation technology uses the selective adsorption of adsorbents to separate substances with similar boiling points. It is characterized by high separation efficiency, low energy consumption, and environmentally friendly process. Adsorbent is the core of adsorption separation technology. USP3510243 uses AgY adsorbent and branched olefins as desorbents. 10 -C 20 Selective adsorption separation of olefins from olefin / alkane mixtures; USP3617504 uses X or Y molecular sieve adsorbents exchanged with copper, potassium, sodium, and silver, and the desorbent is olefin, from C 6 -C 20 Selective adsorption separation of olefins from alkane dehydrogenation products; US20080051619A1 discloses a method for separating olefins from C 9 -C 20 In the method of separating olefins from alkane / olefin mixtures by adsorption, NaX is the first choice of adsorbent. However, since olefins are relatively active, isomerization and polymerization reactions are more likely to occur on molecular sieve adsorbents, resulting in reduced product purity. Polymerization reactions in the micropores of the molecular sieve may also cause the adsorbent to deactivate. USP3718580 proposed that NaX molecular sieves have certain catalytic activity for olefins. This patent uses alkaline Cu 2+ Solution exchange NaX molecular sieve, and then with olefins and Cu + The solution is treated at 172°C to obtain a Cu-exchanged X molecular sieve with high selectivity and low reactivity, but the preparation method of this adsorbent is relatively complicated and costly. Summary of the invention
[0005] The purpose of the present disclosure is to provide an alkane-olefin separation adsorbent and a preparation method and application thereof. The adsorbent has a high adsorption capacity and can obtain a high olefin adsorption selectivity when used for the adsorption separation of alkanes and olefins, and has a low catalytic activity for olefins.
[0006] In order to achieve the above-mentioned object, the present disclosure provides, in a first aspect, an alkane-olefin separation adsorbent, wherein the alkane-olefin separation adsorbent comprises a molecular sieve having a faujasite zeolite structure;
[0007] The pH value of the mixed solution obtained by mixing the alkane-olefin separation adsorbent and deionized water in a volume ratio of 1:1 is 11.0-13.0;
[0008] The water content of the alkane-olefin separation adsorbent is less than 1 weight %.
[0009] Optionally, the pH value of the mixed solution is 12.0-13.0.
[0010] Optionally, the water content of the alkane-olefin separation adsorbent is less than 0.5 wt %.
[0011] Optionally, the particle size of the alkane-olefin separation adsorbent is 0.28-1.0 mm, and the micropore volume is 0.28-0.31 cm 3 / g.
[0012] Optionally, the alkane-olefin separation adsorbent further comprises a non-molecular sieve component;
[0013] Relative to the total weight of the alkane-olefin separation adsorbent, the content of the molecular sieve is 95-100% by weight, and the content of the non-molecular sieve component is 0-5% by weight;
[0014] Optionally, the molecular sieve having a faujasite structure includes NaY molecular sieve and / or NaX molecular sieve;
[0015] Optionally, the non-molecular sieve component comprises SiO 2 and / or Al 2 O 3 .
[0016] A second aspect of the present disclosure provides a method for preparing an alkane-olefin separation adsorbent, the method comprising the following steps:
[0017] (1) mixing a molecular sieve raw material, a binder and an auxiliary agent and performing a molding process to obtain a first product;
[0018] (2) heat treating the first product to obtain a second product;
[0019] (3) mixing a mixed solution comprising an alkali source, an optional silicon source, and an optional aluminum source with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0020] (4) washing the third product until the pH value of the washed liquid is 11.5-13.5 to obtain a fourth product;
[0021] (5) subjecting the fourth product to an activation treatment;
[0022] The molecular sieve raw material includes NaY molecular sieve raw powder and / or NaX molecular sieve raw powder;
[0023] The temperature of the activation treatment is 400-700°C.
[0024] Optionally, in step (1), the binder includes one or more of a clay binder, silica sol and alumina sol;
[0025] The clay binder includes one or more of kaolin, halloysite and attapulgite;
[0026] The auxiliary agent includes one or more of lignin, sesbania powder, corn starch, bayberry tannin and methyl cellulose;
[0027] Optionally, the silicon-aluminum ratio of the NaX molecular sieve raw powder is 2.0-3.0, and the silicon-aluminum ratio of the NaY molecular sieve raw powder is 3.0-6.0.
[0028] Optionally, in step (1), on a dry basis, the weight ratio of the molecular sieve raw material to the binder is (80-95):(5-20);
[0029] On a dry basis, the amount of the auxiliary agent used is 1-5% by weight relative to the total weight of the molecular sieve raw material and the binder.
[0030] Optionally, step (1) further comprises: forming the product of the molding process into particles with a particle size of 0.28-1.0 mm, and performing a first drying process on the particles to obtain the first product;
[0031] Preferably, the particle size of the particles is 0.30-0.85 mm;
[0032] The conditions of the first drying treatment include: temperature of 80-200° C. and time of 2-4 hours.
[0033] Optionally, in step (2), the heat treatment conditions include: temperature of 500-700°C and time of 2-4h.
[0034] Optionally, in step (3), the alkali source includes one or more of NaOH, KOH, RbOH and CsOH;
[0035] The silicon source includes sodium silicate and / or silica sol;
[0036] The aluminum source includes sodium metaaluminate and / or aluminum sol;
[0037] Optionally, in the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon element is (0.6-6.7):1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is (4.0-10.8): 1; H 2 O and Na 2 The molar ratio of sodium element in terms of O is (55-220):1;
[0038] Preferably, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon element is (1.0-5.0):1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is (6.0-8.0):1; 2 O and Na 2 The molar ratio of sodium element based on O is (70-150):1.
[0039] Optionally, in step (3), the aging treatment conditions include: time of 1-24h, temperature of 30-60°C;
[0040] The conditions of the crystallization treatment include: a time of 1-12 hours and a temperature of above 80°C.
[0041] Optionally, in step (4), the pH value of the washed liquid is 12.5-13.5.
[0042] Optionally, step (5) comprises: subjecting the fourth product to a second drying treatment, and then subjecting the fourth product to the activation treatment;
[0043] The conditions of the second drying treatment include: time of 2-5h, temperature of 80-200°C;
[0044] Optionally, the activation treatment time is 2-4 hours.
[0045] The third aspect of the present disclosure provides use of the alkane-olefin separation adsorbent described in the first aspect of the present disclosure in separation of alkanes and olefins.
[0046] Through the above technical scheme, the present invention discloses an adsorbent comprising a molecular sieve with a faujasite structure having specific properties and water content, prepared by molding the molecular sieve, auxiliary agent and binder, heat treatment, binder crystallization, a water washing process with controlled pH value and an activation treatment. The adsorbent has a high adsorption capacity and, when used for the adsorptive separation of alkanes and olefins, has the effects of high olefin adsorption selectivity and low olefin catalytic reaction activity, and is particularly suitable for the separation of alkanes and olefins having the same or similar carbon atom numbers.
[0047] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0049] Figure 1 It is the concentration spectrum of each component in the effluent of the pulse test in Example 1 of the present disclosure. DETAILED DESCRIPTION
[0050] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0051] A first aspect of the present disclosure provides an alkane-olefin separation adsorbent, the alkane-olefin separation adsorbent comprising a molecular sieve having a faujasite zeolite structure;
[0052] The pH value of the mixed solution obtained by mixing the alkane-olefin separation adsorbent and deionized water in a volume ratio of 1:1 is 11.0-13.0;
[0053] The water content of the alkane-olefin separation adsorbent is less than 1 weight %.
[0054] In the present disclosure, the pH value is a test value under normal temperature (25° C.).
[0055] In the present disclosure, "the water content of the alkane-olefin separation adsorbent" refers to the content of water relative to the total weight of the separation adsorbent.
[0056] According to one embodiment of the present disclosure, the pH value of the mixed solution is 12.0-13.0.
[0057] According to one embodiment of the present disclosure, the water content of the alkane-olefin separation adsorbent is less than 0.5 wt %. When the water content of the separation adsorbent is within the range of the present disclosure, a higher olefin adsorption selectivity can be obtained, and polymerization and isomerization reactions of olefins can be avoided.
[0058] According to one embodiment of the present disclosure, the average particle size of the alkane-olefin separation adsorbent is 0.28-1.0 mm, preferably 0.30-0.85 mm; the micropore volume is 0.28-0.31 cm 3 / g.
[0059] According to one embodiment of the present disclosure, the alkane-olefin separation adsorbent further comprises a non-molecular sieve component; relative to the total weight of the alkane-olefin separation adsorbent, the content of the molecular sieve is 95-100% by weight, and the content of the non-molecular sieve component is 0-5% by weight.
[0060] According to one embodiment of the present disclosure, the molecular sieve having a faujasite structure is conventional in the art, for example, includes NaY molecular sieve and / or NaX molecular sieve. When the separation adsorbent contains both NaY molecular sieve and NaX molecular sieve, the ratio of the two is not limited, that is, any ratio of NaY molecular sieve and NaX molecular sieve can realize the technical solution of the present disclosure.
[0061] According to one embodiment of the present disclosure, the non-molecular sieve component includes SiO 2 and / or Al 2 O 3 .
[0062] A second aspect of the present disclosure provides a method for preparing an alkane-olefin separation adsorbent, the method comprising the following steps:
[0063] (1) mixing a molecular sieve raw material, a binder and an auxiliary agent and performing a molding process to obtain a first product;
[0064] (2) heat treating the first product to obtain a second product;
[0065] (3) mixing a mixed solution comprising an alkali source, an optional silicon source, and an optional aluminum source with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0066] (4) washing the third product until the pH value of the washed liquid is 11.5-13.5 to obtain a fourth product;
[0067] (5) subjecting the fourth product to an activation treatment;
[0068] The molecular sieve raw material includes NaY molecular sieve raw powder and / or NaX molecular sieve raw powder;
[0069] The temperature of the activation treatment is 400-700°C.
[0070] According to one embodiment of the present disclosure, in step (1), the binder includes one or more of a clay binder, silica sol and alumina sol; the clay binder includes one or more of kaolin, halloysite and attapulgite; the auxiliary agent includes one or more of lignin, sesbania powder, corn starch, bayberry tannin extract and methyl cellulose.
[0071] According to one embodiment of the present disclosure, the silicon-aluminum ratio of the NaX molecular sieve raw powder is 2.0-3.0, and the silicon-aluminum ratio of the NaY molecular sieve raw powder is 3.0-6.0; wherein the silicon-aluminum ratio refers to the SiO 2 With Al 2 O 3 The molar ratio of silicon to aluminum can improve the adsorption selectivity of the adsorbent for olefins.
[0072] According to one embodiment of the present disclosure, in step (1), on a dry basis, the weight ratio of the molecular sieve raw material to the binder is (80-95): (5-20), preferably (90-95): (5-10). When the weight ratio of the molecular sieve raw material to the binder is within the above range, the problems of high bulk density of the adsorbent due to excessively high binder content, decreased active component content, and poor adsorbent strength due to too low a binder content can be avoided.
[0073] According to one embodiment of the present disclosure, in step (1), the amount of the auxiliary agent used is 1-5% by weight, preferably 2-4% by weight, relative to the total weight of the molecular sieve raw material and the binder, calculated on a dry basis.
[0074] In the present disclosure, the molding process may be, for example, rolling ball molding, extrusion molding or tablet molding, and the molding process may be performed in a high-speed granulator, sugar coating machine, disc granulator, extruder, tablet press and other equipment. For example, rolling ball molding may be performed by placing the mixed powder into a rolling ball device, adding water to the material in the form of spraying while rolling, and adding the mixed powder into the material in the form of scattering, so that the fine powder agglomerates, becomes round, and forms small balls, and then scatters to obtain spherical particles; extrusion molding may be performed by placing the mixed powder into an extrusion device, first kneading by adding a certain amount of water, and then extruding to obtain strips, and drying, crushing and sieving the strips to obtain particles; tablet molding may be performed by placing the mixed powder into a tablet press device, pressing and molding, and then crushing and sieving to obtain particles.
[0075] According to one embodiment of the present disclosure, step (1) further comprises: forming the product of the molding process into particles with a particle size of 0.28-1.0 mm, performing a first drying process on the particles to obtain a first product, wherein the particle size of the particles is preferably 0.30-0.85 mm, and the particles are preferably spherical particles, which have good fluidity, are easy to be filled evenly, and have good fluid distribution uniformity; the conditions of the first drying process include: a temperature of 80-200° C. and a time of 2-4 hours. The first drying method is conventional in the art and is not specifically required.
[0076] According to one embodiment of the present disclosure, the temperature of the activation treatment is 500-700°C.
[0077] According to one embodiment of the present disclosure, in step (2), the heat treatment conditions include: a temperature of 500-700°C and a time of 2-4 hours. When the binder used includes a clay binder, such as one or more of kaolin, halloysite and attapulgite, the heat treatment can convert it into a reactive aluminosilicate, which, together with silica sol and alumina sol, can enhance the strength of the particles, prevent pulverization during crystallization, and can cause the additive to burn and decompose, forming a pore structure inside the separation adsorbent, improving mass transfer performance, and enhancing the adsorption capacity for olefins.
[0078] According to one embodiment of the present disclosure, the alkali source includes one or more of NaOH, KOH, RbOH and CsOH; the silicon source includes sodium silicate and / or silica sol; and the aluminum source includes sodium aluminate and / or aluminum sol.
[0079] According to one embodiment of the present disclosure, in the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon element is (0.6-6.7):1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is (4.0-10.8): 1; H 2 O and Na 2 The molar ratio of sodium element in terms of O is (55-220):1; preferably, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon element is (1.0-5.0):1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is (6.0-8.0):1; 2 O and Na 2The molar ratio of sodium element to NaX element is (70-150): 1. The above feed ratio can make the binder easier to be converted into NaX and / or NaY molecular sieve.
[0080] According to an embodiment of the present disclosure, in step (3), the conditions of the aging treatment include: time of 1-24 hours, preferably 4-12 hours; temperature of 30-60° C., preferably 40-50° C.; conditions of the crystallization treatment include: time of 1-12 hours, preferably 2-8 hours, more preferably 2.5-4 hours; temperature of 80° C. or above, preferably 85-100° C., more preferably 90-95° C. The aging treatment and crystallization treatment can convert at least part of the amorphous silicon aluminum in the second product into NaY molecular sieve and / or NaX molecular sieve.
[0081] According to one embodiment of the present disclosure, step (4) comprises: washing the third product with water until the pH value of the washed liquid is 11.5-13.5, wherein the water is preferably deionized water.
[0082] In the present disclosure, if the pH value of the washed liquid in step (4) is less than 11.5, the fourth product can be soaked in a 0.05-0.10 mol / L NaOH solution until the pH value of the washed liquid reaches 11.5-13.5, and then step (5) can be performed.
[0083] According to one embodiment of the present disclosure, in step (4), the pH value of the washed liquid is 12.5-13.5.
[0084] According to one embodiment of the present disclosure, step (5) includes: subjecting the fourth product to a second drying treatment and then to an activation treatment; the conditions for the second drying treatment include: a time of 2-5 hours, preferably 3-4 hours; a temperature of 80-200°C, preferably 100-150°C.
[0085] According to one embodiment of the present disclosure, the activation treatment time is 2-4 hours. The activation treatment can be carried out in a dry compressed air atmosphere, or in a vacuum condition, or in a nitrogen atmosphere.
[0086] The third aspect of the present disclosure provides use of the alkane-olefin separation adsorbent described in the first aspect of the present disclosure in separation of alkanes and olefins.
[0087] Unless otherwise specified, the reagents used in the examples and comparative examples are commercially available.
[0088] Gas chromatography instrument model and test conditions: Agilent GC6890 gas chromatograph was used, the chromatographic column was model HP-5, the injection volume was 0.3 μL, the injection port temperature was 290°C, the split ratio was 100:1, FID detection, the detector temperature was 290°C, the initial column temperature was 50°C, maintained for 20 min, increased to 250°C at 2°C / min, and maintained for 5 min.
[0089] Static equilibrium test method: prepare a solution with a composition of 90 weight % n-dodecane and 10 weight % 1-dodecene, weigh 12 g of the above solution and 3 g of adsorbent and place them in a 25 mL autoclave, then put the autoclave into an oven and keep it at 135°C for 20 hours. After cooling, take the supernatant and use gas chromatography to analyze the composition of the sample after static equilibrium, and add the mass fractions of the newly generated impurities. The larger the value after the addition, the greater the degree of reaction.
[0090] In the following examples and comparative examples, the masses of molecular sieves and binders are all dry basis masses, the toluene adsorption capacity of the molecular sieve raw powder used is 232 mg / g, the molar ratio of silica to alumina of the kaolin and halloysite used is 1.9, and the molar ratio of silica to alumina of the attapulgite used is 8.0.
[0091] Method for determining the toluene adsorption of the adsorbent sample: Take 1g of sample and activate it at 500℃ for 2h, then cool it to room temperature in a desiccator. The net weight of the sample is M 0 Then, the sample was saturated with a mixture of nitrogen and toluene vapor at 35°C. The total pressure of the mixed gas was 0.1 MPa, of which the partial pressure of toluene vapor was 0.5 times the saturated vapor pressure of toluene at that temperature. The net weight of the sample after saturation was M 1 , then the toluene adsorption of the sample (mg / g) = 1000×(M 1 -M 0 ) / M 0 The molecular sieve content in the adsorbent can be expressed by the ratio of the toluene adsorption amount of the adsorbent to the toluene adsorption amount of the molecular sieve raw powder.
[0092] The mechanical strength of the adsorbent is characterized by the compressive crushing rate. The determination method is: take an appropriate amount of adsorbent at a constant weight in the air, weigh it and put it into a stainless steel cylinder with a closed bottom, place a cylindrical ejector pin that matches the stainless steel cylinder on the top of the adsorbent, and then place it on a particle strength tester to pressurize the ejector pin to 130N, release the pressure and take out the adsorbent, sieve it with a 0.3mm mesh, weigh the small balls that do not pass through the sieve, and the percentage of the reduced mass to the mass of the sample before pressurization is the compressive crushing rate of the tested sample. The lower the crushing rate, the better the strength of the sample.
[0093] The method for determining the ignition density of the adsorbent is as follows: take an appropriate amount of the adsorbent at a constant weight in air, put it into a glass measuring cylinder, place it on a tap density meter and vibrate it for 5 minutes, then read the volume number V, where the amplitude is 3mm and the vibration frequency is 290 times / min. Then weigh the net weight M of the sample, and then take an appropriate amount of the sample to test its mass ignition loss rate K (%) after calcination at 600℃ for 2h, which is the water content. The ignition density of the adsorbent (g / mL) = M×(1-K) / V.
[0094] Particle size testing method: Take an appropriate amount of adsorbent at a constant weight in the air, and place it tightly from top to bottom according to 20-mesh and 50-mesh standard sieves (corresponding mesh sizes are 0.85mm and 0.3mm respectively) and collection plates, put the adsorbent sample with a mass of M on the 20-mesh sieve, and then sieve it on an automatic sieve vibrator with an amplitude of 0.8mm and a vibration time of 3min. The particles obtained on the 50-mesh sieve are particles with a size of 20 mesh (0.85mm) to 50 mesh (0.3mm), that is, particles with a size of 0.30-0.85mm.
[0095] Testing method for micropore volume: nitrogen adsorption BET method.
[0096] The separation adsorbent prepared in the embodiment and the comparative example is composed of molecular sieve and non-molecular sieve components. When the binder is a clay binder and the non-molecular sieve is composed of SiO 2 and Al 2 O 3 ; When the binder is silica sol and the non-molecular sieve component is SiO 2 ; When the binder is aluminum sol and the non-molecular sieve component is Al 2 O 3 .
[0097] Example 1
[0098] The following steps were used to prepare the alkane-olefin separation adsorbent X-1:
[0099] (1) 95 kg of NaX molecular sieve powder with a silicon-aluminum ratio of 2.2, 5 kg of kaolin and 2 kg of sesbania powder are uniformly mixed to form a mixed powder, and the mixed powder is rolled into balls in a rotary high-speed granulator. During the rolling process, deionized water is sprayed into the material and the mixed powder is sprinkled, and spherical particles with a particle size of 0.30-0.85 mm are sieved;
[0100] On a dry basis, the weight ratio of the NaX molecular sieve raw powder to the kaolin is 95:5, and the amount of the sesbania powder is 2% by weight relative to the total weight of the NaX molecular sieve raw powder and the kaolin;
[0101] The spherical particles are subjected to a first drying treatment to obtain a first product; the conditions of the first drying treatment include: a time of 4 hours and a temperature of 100° C.;
[0102] (2) calcining the first product to obtain a second product; the calcination temperature is 540° C. and the time is 4 h;
[0103] (3) mixing a mixed solution containing sodium aluminate, sodium silicate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0104] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon element is 0.6:1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 4.0:1; 2 O and Na 2 The molar ratio of sodium element in O is 55:1;
[0105] The conditions of aging treatment included: temperature of 40°C and time of 5 h;
[0106] The conditions of the crystallization treatment include: temperature of 91°C and time of 4 h;
[0107] (4) washing the third product with deionized water until the pH value of the washed solution is 13.5, thereby obtaining a fourth product;
[0108] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent X-1;
[0109] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0110] The activation treatment was carried out in a dry air atmosphere at a temperature of 700°C for 2 h. The parameters of the separation adsorbent X-1 are listed in Tables 1 and 2.
[0111] Example 2
[0112] The following steps were used to prepare the alkane-olefin separation adsorbent X-2:
[0113] (1) 80 kg of NaY molecular sieve powder with a silicon-aluminum ratio of 6.0, 20 kg of attapulgite and 4 kg of corn starch were uniformly mixed to form a mixed powder, 50 kg of deionized water was added, the mixture was put into a kneader and kneaded for 30 min, and then extruded into strips in an extruder. After drying, the strips were broken and sieved to obtain particles with a particle size of 0.30-0.85 mm;
[0114] On a dry basis, the weight ratio of the NaY molecular sieve raw powder to the attapulgite is 80:20, and the amount of corn starch used is 4 weight % relative to the total weight of the NaY molecular sieve raw powder and the attapulgite;
[0115] The particles are subjected to a first drying process to obtain a first product; the conditions of the first drying process include: a time of 3 hours and a temperature of 100° C.;
[0116] (2) calcining the first product to obtain a second product; the calcination temperature is 550° C. and the time is 4 h;
[0117] (3) mixing a mixed solution containing sodium metaaluminate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0118] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon is 6.7:1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 10.8:1; 2 O and Na 2 The molar ratio of sodium element in O is 220:1;
[0119] The conditions of aging treatment include: temperature of 50°C and time of 10 h;
[0120] The conditions of the crystallization treatment include: temperature of 95°C and time of 3 h;
[0121] (4) washing the third product with deionized water until the pH value of the washed solution is 13.0, thereby obtaining a fourth product;
[0122] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent X-2;
[0123] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0124] The activation treatment was carried out in a dry air atmosphere at a temperature of 400°C for 2 h. The parameters of the separation adsorbent X-2 are listed in Tables 1 and 2.
[0125] Example 3
[0126] The following steps were used to prepare the alkane-olefin separation adsorbent X-3:
[0127] (1) 90 kg of NaX molecular sieve powder with a silicon-aluminum ratio of 2.8, 5 kg of silica sol and 3 kg of bayberry tannin extract were uniformly mixed to form a mixed powder, which was put into a tablet press for compression molding. After drying, the flakes were crushed and spherical particles with a particle size of 0.30-0.85 mm were obtained by screening;
[0128] On a dry basis, the weight ratio of the NaX molecular sieve raw powder to the kaolin is 90:5, and the amount of the bayberry tannin extract is 3 weight % relative to the total weight of the NaX molecular sieve raw powder and the silica sol;
[0129] The spherical particles are subjected to a first drying treatment to obtain a first product; the conditions of the first drying treatment include: a drying time of 2 hours and a temperature of 100° C.;
[0130] (2) calcining the first product to obtain a second product; the calcination temperature is 550° C. and the time is 4 h;
[0131] (3) mixing a mixed solution containing sodium metaaluminate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0132] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon is 4.3:1, with SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 6.3; 2 O and Na 2 The molar ratio of sodium element in O is 101:1;
[0133] The conditions of aging treatment include: temperature of 50°C and time of 10 h;
[0134] The conditions of the crystallization treatment include: temperature of 95°C and time of 3 h;
[0135] (4) washing the third product with deionized water until the pH value of the washed solution is 12.0, thereby obtaining a fourth product;
[0136] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent X-3;
[0137] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0138] The activation treatment was carried out in a dry air atmosphere at a temperature of 500°C for 2 h. The parameters of the separation adsorbent X-3 are listed in Tables 1 and 2.
[0139] Example 4
[0140] The following steps were used to prepare the alkane-olefin separation adsorbent X-4:
[0141] (1) 47.5 kg of NaX molecular sieve powder with a silicon-aluminum ratio of 2.5, 47.5 kg of NaY molecular sieve powder with a silicon-aluminum ratio of 3.5, 5 kg of aluminum sol and 3 kg of methyl cellulose are uniformly mixed to form a mixed powder, and the mixed powder is rolled into balls in a rotary high-speed granulator. During the rolling process, deionized water is sprayed into the material and the mixed powder is sprinkled, and spherical particles with a particle size of 0.30-0.85 mm are sieved;
[0142] On a dry basis, the weight ratio of the total weight of the NaX molecular sieve raw powder and the NaY molecular sieve raw powder to the aluminum sol is 95:5, and the weight ratio of the NaX molecular sieve raw powder to the NaY molecular sieve raw powder is 1:1; relative to the total weight of the NaX molecular sieve raw powder, the NaY molecular sieve raw powder and the aluminum sol, the amount of methyl cellulose used is 3 weight%;
[0143] The spherical particles are subjected to a first drying treatment to obtain a first product; the conditions of the first drying treatment include: a time of 4 hours and a temperature of 100° C.;
[0144] (2) calcining the first product to obtain a second product; the calcination temperature is 600° C. and the time is 4 h;
[0145] (3) mixing a mixed solution containing sodium aluminate, sodium silicate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0146] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon is 2.3:1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 8.5; 2 O and Na 2 The molar ratio of sodium element in O is 75:1;
[0147] The conditions of aging treatment included: temperature of 40°C and time of 6 h;
[0148] The conditions of the crystallization treatment include: temperature of 98°C and time of 3 h;
[0149] (4) washing the third product with deionized water until the pH value of the washed solution is 12.5, thereby obtaining a fourth product;
[0150] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent X-4;
[0151] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0152] The activation treatment was carried out in a dry air atmosphere at a temperature of 600°C for 2 h. The parameters of the separation adsorbent X-4 are listed in Tables 1 and 2.
[0153] Example 5
[0154] The following steps were used to prepare the alkane-olefin separation adsorbent X-5:
[0155] (1) 95 kg of NaX molecular sieve powder with a silicon-aluminum ratio of 2.5, 5 kg of halloysite and 3 kg of corn starch are uniformly mixed to form a mixed powder, and the mixed powder is rolled into balls in a rotary high-speed granulator. During the rolling process, deionized water is sprayed into the material and the mixed powder is sprinkled, and spherical particles with a particle size of 0.30-0.85 mm are screened;
[0156] On a dry basis, the weight ratio of the NaX molecular sieve raw powder to the kaolin is 95:5, and the amount of corn starch used is 3 weight % relative to the total weight of the NaX molecular sieve raw powder and halloysite;
[0157] The spherical particles are subjected to a first drying treatment to obtain a first product; the conditions of the first drying treatment include: a time of 3 hours and a temperature of 100° C.;
[0158] (2) calcining the first product to obtain a second product; the calcination temperature is 650° C. and the time is 4 h;
[0159] (3) mixing a mixed solution containing sodium aluminate, sodium silicate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0160] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon is 3.2:1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 7.3:1; 2 O and Na 2 The molar ratio of sodium element to O is 150:1;
[0161] The conditions of aging treatment included: temperature of 40°C and time of 6 h;
[0162] The conditions of the crystallization treatment include: temperature of 95°C and time of 3 h;
[0163] (4) washing the third product with deionized water until the pH value of the washed solution is 13.5, thereby obtaining a fourth product;
[0164] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent X-5;
[0165] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0166] The activation treatment was carried out in a dry air atmosphere at a temperature of 550°C for 2 h. The parameters of the separation adsorbent X-5 are listed in Tables 1 and 2.
[0167] Example 6
[0168] The following steps were used to prepare the alkane-olefin separation adsorbent X-6:
[0169] (1) 90 kg of NaX molecular sieve powder with a silicon-aluminum ratio of 2.5, 2.5 kg of kaolin, 2.5 kg of halloysite, 2.5 kg of silica sol, 2 kg of aluminum sol, 1 kg of corn starch, 1 kg of sesbania powder, and 1 kg of bayberry tannin extract are uniformly mixed to form a mixed powder, and the mixed powder is rolled into a ball in a rotary high-speed granulator. During the rolling process, deionized water is sprayed into the material and the mixed powder is scattered, and spherical particles with a particle size of 0.30-0.85 mm are sieved;
[0170] On a dry basis, the weight ratio of the NaX molecular sieve raw powder to the binder is 90:10, and the amount of the sesbania powder is 3 weight % relative to the total weight of the NaX molecular sieve raw powder and the binder;
[0171] The spherical particles are subjected to a first drying treatment to obtain a first product; the conditions of the first drying treatment include: a time of 4 hours and a temperature of 100° C.;
[0172] (2) calcining the first product to obtain a second product; the calcination temperature is 650° C. and the time is 5 h;
[0173] (3) mixing a mixed solution containing sodium aluminate, sodium silicate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0174] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon element is 1.5:1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 5.2:1; 2 O and Na 2 The molar ratio of sodium element in O is 90:1;
[0175] The conditions of aging treatment included: temperature of 40°C and time of 6 h;
[0176] The conditions of the crystallization treatment include: temperature of 98°C and time of 3 h;
[0177] (4) washing the third product with deionized water until the pH value of the washed solution is 13.0, thereby obtaining a fourth product;
[0178] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent X-6;
[0179] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0180] The activation treatment was carried out in a dry air atmosphere at a temperature of 500°C for 2 h. The parameters of the separation adsorbent X-6 are listed in Tables 1 and 2.
[0181] Comparative Example 1
[0182] The following steps were used to prepare the alkane-olefin separation adsorbent Y-1:
[0183] (1) 95 kg of NaX molecular sieve powder with a silicon-aluminum ratio of 2.2, 5 kg of kaolin and 2 kg of sesbania powder are uniformly mixed to form a mixed powder, and the mixed powder is rolled into balls in a rotary high-speed granulator. During the rolling process, deionized water is sprayed into the material and the mixed powder is sprinkled, and spherical particles with a particle size of 0.30-0.85 mm are sieved;
[0184] On a dry basis, the weight ratio of the NaX molecular sieve raw powder to the kaolin is 95:5, and the amount of the sesbania powder is 2 weight % relative to the total weight of the NaX molecular sieve raw powder and the kaolin;
[0185] The spherical particles are subjected to a first drying treatment to obtain a first product; the conditions of the first drying treatment include: a time of 8 hours and a temperature of 100° C.;
[0186] (2) The first product was calcined to obtain separation adsorbent Y-1; the calcination temperature was 700°C and the time was 4 hours; the parameters of separation adsorbent Y-1 are listed in Tables 1 and 2.
[0187] Comparative Example 2
[0188] The separation adsorbent Y-2 was prepared by the following steps:
[0189] (1) 80 kg of NaY molecular sieve powder with a silicon-aluminum ratio of 6.0, 20 kg of attapulgite and 4 kg of corn starch were uniformly mixed to form a mixed powder, 50 kg of deionized water was added, the mixture was put into a kneader and kneaded for 30 min, and then extruded into strips in an extruder. After drying, the strips were broken and sieved to obtain particles with a particle size of 0.30-0.85 mm;
[0190] On a dry basis, the weight ratio of the NaY molecular sieve raw powder to the attapulgite is 80:20, and the amount of corn starch used is 4 weight % relative to the total weight of the NaY molecular sieve raw powder and the attapulgite;
[0191] The particles are subjected to a first drying process to obtain a first product; the conditions of the first drying process include: a time of 3 hours and a temperature of 100° C.;
[0192] (2) calcining the first product to obtain a second product; the calcination temperature is 550° C. and the time is 4 h;
[0193] (3) mixing a mixed solution containing sodium metaaluminate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0194] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon is 6.7:1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 10.8:1; 2 O and Na 2 The molar ratio of sodium element in O is 220:1;
[0195] The conditions of aging treatment include: temperature of 50°C and time of 10 h;
[0196] The conditions of the crystallization treatment include: temperature of 95°C and time of 3 h;
[0197] (4) washing the third product with deionized water until the pH value of the washed solution is 9.0, thereby obtaining a fourth product;
[0198] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent Y-2;
[0199] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0200] The activation treatment was carried out in a dry air atmosphere at a temperature of 400°C for 2 h. The parameters of the separation adsorbent Y-2 are listed in Tables 1 and 2.
[0201] Comparative Example 3
[0202] The following steps were used to prepare the alkane-olefin separation adsorbent Y-3:
[0203] (1) 95 kg of NaX molecular sieve powder with a silicon-aluminum ratio of 2.5, 5 kg of halloysite and 3 kg of corn starch are uniformly mixed to form a mixed powder, and the mixed powder is rolled into balls in a rotary high-speed granulator. During the rolling process, deionized water is sprayed into the material and the mixed powder is sprinkled, and spherical particles with a particle size of 0.30-0.85 mm are screened;
[0204] On a dry basis, the weight ratio of the NaX molecular sieve raw powder to the kaolin is 95:5, and the amount of corn starch used is 3 weight % relative to the total weight of the NaX molecular sieve raw powder and halloysite;
[0205] The spherical particles are subjected to a first drying treatment to obtain a first product; the conditions of the first drying treatment include: a time of 3 hours and a temperature of 100° C.;
[0206] (2) calcining the first product to obtain a second product; the calcination temperature is 650° C. and the time is 4 h;
[0207] (3) mixing a mixed solution containing sodium aluminate, sodium silicate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0208] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon is 3.2:1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 7.3:1; 2 O and Na 2 The molar ratio of sodium element to O is 150:1;
[0209] The conditions of aging treatment included: temperature of 40°C and time of 6 h;
[0210] The conditions of the crystallization treatment include: temperature of 95°C and time of 3 h;
[0211] (4) washing the third product with deionized water until the pH value of the washed solution is 13.5, thereby obtaining a fourth product;
[0212] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent Y-3;
[0213] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0214] The activation treatment was carried out in a dry air atmosphere at a temperature of 250°C for 2 h. The parameters of the separation adsorbent Y-3 are listed in Tables 1 and 2.
[0215] Comparative Example 4
[0216] The separation adsorbent Y-4 was prepared by the following steps:
[0217] (1) 80 kg of NaY molecular sieve powder with a silicon-aluminum ratio of 6.0, 20 kg of attapulgite and 4 kg of corn starch were uniformly mixed to form a mixed powder, 50 kg of deionized water was added, the mixture was put into a kneader and kneaded for 30 min, and then extruded into strips in an extruder. After drying, the strips were broken and sieved to obtain particles with a particle size of 0.30-0.85 mm;
[0218] On a dry basis, the weight ratio of the NaY molecular sieve raw powder to the attapulgite is 80:20, and the amount of corn starch used is 4 weight % relative to the total weight of the NaY molecular sieve raw powder and the attapulgite;
[0219] The particles are subjected to a first drying process to obtain a first product; the conditions of the first drying process include: a time of 3 hours and a temperature of 100° C.;
[0220] (2) calcining the first product to obtain a second product; the calcination temperature is 550° C. and the time is 4 h;
[0221] (3) mixing a mixed solution containing sodium metaaluminate and NaOH with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product;
[0222] In the mixture, Na 2 Sodium in terms of O and SiO 2 The molar ratio of silicon is 6.7:1, SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 10.8:1; 2 O and Na 2 The molar ratio of sodium element in O is 220:1;
[0223] The conditions of aging treatment include: temperature of 50°C and time of 10 h;
[0224] The conditions of the crystallization treatment include: temperature of 95°C and time of 3 h;
[0225] (4) washing the third product with deionized water until the pH value of the washed solution is 14.5, thereby obtaining a fourth product;
[0226] (5) subjecting the fourth product to a second drying treatment and an activation treatment to obtain a separation adsorbent Y-2;
[0227] The conditions of the second drying treatment include: temperature of 100°C and time of 4h;
[0228] The activation treatment was carried out in a dry air atmosphere at a temperature of 400°C for 2 h. The parameters of the separation adsorbent Y-4 are listed in Tables 1 and 2.
[0229] Test Example 1
[0230] The separation degree test of the separation adsorbent prepared in the embodiment and the comparative example was carried out by using the pulse test method, as follows:
[0231] The pulse experiment device consists of a feed system, a nitrogen system, an adsorption column, a heating box, a pressure control valve, a micro plunger pump, etc. The adsorption column is a stainless steel coil of φ8mm×1mm and 2300mm long, with an adsorbent loading of about 65mL, placed in an automatic temperature-controlled heating box. The feed system at the inlet end of the adsorption column is connected to the nitrogen system, and the outlet end is connected to a back pressure valve and then to the effluent collector.
[0232] The desorption liquid composition was 50 wt% 1-hexene and 50 wt% n-hexane.
[0233] The raw materials to be separated consist of 5% by weight each of n-decane, 1-decene, n-undecane, 1-undecene, n-dodecane, 1-dodecene, n-tridecane, 1-tridecene, n-tetradecane, 1-tetradecene and 50% by weight of isooctane.
[0234] The volume ratio of the separation adsorbent to the raw material to be separated is 8.125:1.
[0235] The separation adsorbent is loaded into the adsorption column and filled, and the desorption liquid is injected with a plunger pump. When the composition of the outlet material is stable, the desorption liquid is stopped, 8 mL of the raw material to be separated is injected, and then the desorption liquid is used for elution at a rate of 1.5 mL / min. At the beginning of elution, about 0.1 mL of the desorption sample is taken for every 2 mL at the outlet of the adsorption column until the components in the raw material to be separated are completely desorbed, that is, the effluent of the adsorption column does not contain the components in the raw material to be separated.
[0236] The composition of the sample was analyzed by gas chromatography. The volume of the desorption liquid during elution was used as the horizontal coordinate, and the mass fraction of n-decane, 1-decene, n-undecane, 1-undecene, n-dodecane, 1-dodecene, n-tridecane, 1-tridecene, n-tetradecane and 1-tetradecene was used as the vertical coordinate to draw the envelope curve of the above components. n-Decane, n-undecane, n-dodecane, n-tridecane and n-tetradecane are weakly adsorbed and are eluted first, and the peaks are almost at the same time. The volume of the desorption liquid corresponding to the peak of each of the above alkanes is the retention volume V R; 1-decene, 1-undecene, 1-dodecene, 1-tridecene and 1-tetradecene are subsequently eluted and peaks appear in sequence, and the retention volumes of 1-decene, 1-undecene, 1-dodecene, 1-tridecene and 1-tetradecene are respectively subtracted from the retention volumes of n-decane, n-undecane, n-dodecane, n-tridecane and n-tetradecane to obtain the net retention volumes ΔV of 1-decene, 1-undecene, 1-dodecene, 1-tridecene and 1-tetradecene. R .W 1 / 2 It represents the half-peak width of the mass fraction curve of each component. Figure 1 It is the concentration spectrum of each component in the effluent of Example 1.
[0237] The resolution (R) also takes into account ΔV R and W 1 / 2 R can be used to reflect the separation effect between an olefin and an alkane with the same carbon number. The larger the separation degree R, the better the adsorption separation effect. R = 2ΔV Ra / (W 1 / 2a +W 1 / 2b ), where ΔV Ra is the net retention volume of an olefin relative to an alkane with the same carbon number, W 1 / 2a and W 1 / 2b are the half peak widths of the olefin and the alkane with the same carbon number, respectively. The results are listed in Table 3.
[0238] The boiling point of n-hexane in the desorption liquid is 69°C, the boiling point of 1-hexene is 62.8°C, and the boiling point of the first olefin composed of 1-decene, 1-undecene, 1-dodecene, 1-tridecene and 1-tetradecene is 169-171°C.
[0239] Table 1
[0240]
[0241]
[0242] Table 2
[0243]
[0244] Table 3
[0245]
[0246] According to the data in Table 2, when the separation adsorbent prepared by the method disclosed in the present invention is used for the adsorption separation of alkanes and alkenes, the static equilibrium impurity mass fraction is small, indicating that the degree of isomerization or polymerization reaction of the olefins is small.
[0247] According to the data in Table 3, when the separation adsorbent prepared by the method disclosed in the present invention is used for the adsorption separation of alkanes and alkenes, the separation degree is relatively large, indicating that the separation effect of alkenes and alkanes with the same carbon number is better.
[0248] Furthermore, according to the data of Examples 3 and 5, when the pH value of the washed liquid in step (4) is within the preferred range of 12.5-13.5, the prepared separation adsorbent has a better adsorption and separation effect.
[0249] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0250] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0251] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. An alkane-olefin separation adsorbent, characterized in that: The alkane-olefin separation adsorbent comprises a molecular sieve having a faujasite zeolite structure; The pH value of the mixed solution obtained by mixing the alkane-olefin separation adsorbent and deionized water in a volume ratio of 1:1 is 11.0-13.0; The water content of the alkane-olefin separation adsorbent is less than 1 weight %.
2. The alkane-olefin separation adsorbent according to claim 1, wherein: The pH value of the mixed solution is 12.0-13.
0.
3. The alkane-olefin separation adsorbent according to claim 1, wherein: The water content of the alkane-olefin separation adsorbent is less than 0.5 wt %.
4. The alkane-olefin separation adsorbent according to claim 1, wherein: The particle size of the alkane-olefin separation adsorbent is 0.28-1.0 mm, and the micropore volume is 0.28-0.31 cm 3 / g.
5. The alkane-olefin separation adsorbent according to claim 1, wherein: The alkane-olefin separation adsorbent further comprises a non-molecular sieve component; Relative to the total weight of the alkane-olefin separation adsorbent, the content of the molecular sieve is 95-100% by weight, and the content of the non-molecular sieve component is 0-5% by weight; Optionally, the molecular sieve having a faujasite structure includes NaY molecular sieve and / or NaX molecular sieve; Optionally, the non-molecular sieve component includes SiO2 and / or Al2O3.
6. A method for preparing the alkane-olefin separation adsorbent according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) mixing a molecular sieve raw material, a binder and an auxiliary agent and performing a molding process to obtain a first product; (2) heat treating the first product to obtain a second product; (3) mixing a mixed solution comprising an alkali source, an optional silicon source, and an optional aluminum source with the second product, and subjecting the obtained mixture to an aging treatment and a crystallization treatment to obtain a third product; (4) washing the third product until the pH value of the washed liquid is 11.5-13.5 to obtain a fourth product; (5) subjecting the fourth product to an activation treatment; The molecular sieve raw material includes NaY molecular sieve raw powder and / or NaX molecular sieve raw powder; The temperature of the activation treatment is 400-700°C.
7. The method according to claim 6, wherein: In step (1), the binder includes one or more of a clay binder, silica sol and alumina sol; The clay binder includes one or more of kaolin, halloysite and attapulgite; The auxiliary agent includes one or more of lignin, sesbania powder, corn starch, bayberry tannin and methyl cellulose; Optionally, the silicon-aluminum ratio of the NaX molecular sieve raw powder is 2.0-3.0, and the silicon-aluminum ratio of the NaY molecular sieve raw powder is 3.0-6.
0.
8. The method according to claim 6, wherein: In step (1), the weight ratio of the molecular sieve raw material to the binder is (80-95): (5-20) on a dry basis; On a dry basis, the amount of the auxiliary agent used is 1-5% by weight relative to the total weight of the molecular sieve raw material and the binder.
9. The method according to claim 6, wherein: Step (1) further includes: forming the product of the molding process into particles with a particle size of 0.28-1.0 mm, and performing a first drying process on the particles to obtain the first product; Preferably, the particle size of the particles is 0.30-0.85 mm; The conditions of the first drying treatment include: temperature of 80-200° C. and time of 2-4 hours.
10. The method according to claim 6, wherein: In step (2), the heat treatment conditions include: temperature of 500-700°C and time of 2-4h.
11. The method according to claim 6, wherein: In step (3), the alkali source includes one or more of NaOH, KOH, RbOH and CsOH; The silicon source includes sodium silicate and / or silica sol; The aluminum source includes sodium metaaluminate and / or aluminum sol; Optionally, in the mixture, the molar ratio of sodium element calculated as Na2O to silicon element calculated as SiO2 is (0.6-6.7):1, the molar ratio of silicon element calculated as SiO2 to aluminum element calculated as Al2O3 is (4.0-10.8):1; the molar ratio of H2O to sodium element calculated as Na2O is (55-220):1; Preferably, the molar ratio of sodium element calculated as Na2O to silicon element calculated as SiO2 is (1.0-5.0):1, the molar ratio of silicon element calculated as SiO2 to aluminum element calculated as Al2O3 is (6.0-8.0):1; the molar ratio of H2O to sodium element calculated as Na2O is (70-150):
1.
12. The method according to claim 6, wherein: In step (3), the aging treatment conditions include: time of 1-24h, temperature of 30-60°C; The conditions of the crystallization treatment include: a time of 1-12 hours and a temperature of above 80°C.
13. The method according to claim 6, wherein: In step (4), the pH value of the washed liquid is 12.5-13.
5.
14. The method according to claim 6, wherein: Step (5) comprises: subjecting the fourth product to a second drying treatment, and then subjecting the fourth product to the activation treatment; The conditions of the second drying treatment include: time of 2-5h, temperature of 80-200°C; Optionally, the activation treatment time is 2-4 hours.
15. Use of the alkane-olefin separation adsorbent according to any one of claims 1 to 5 in the separation of alkanes and olefins.
Citation Information
Patent Citations
Preparation method of m-xylene adsorbent
CN111097372A
Olefine separation method
CN1339425A
X-type zeolite molded body and its production