Preparation method and application of TEA aminated UiO-66 porous material
The preparation of TEA aminated UiO-66 porous materials solves the problems of insufficient stability of metal-organic framework materials in the process of adsorbing hydrogen sulfide and low removal efficiency of low-concentration hydrogen sulfide, and achieves efficient hydrogen sulfide adsorption and deep desulfurization capabilities. , suitable for hydrogen sulfide control.
Patent Information
- Application Number
- CN202410829468.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-22
AI Technical Summary
Existing metal-organic framework materials have insufficient stability during the adsorption of hydrogen sulfide, resulting in pore collapse, and low removal efficiency of low-concentration hydrogen sulfide, making it impossible to effectively achieve deep desulfurization.
The TEA aminated UiO-66 porous material preparation method is used. Through hydrothermal reaction and activation treatment, amino functional groups are introduced to enhance the interaction between the adsorbent and the adsorbent and improve the adsorption kinetic performance.
The prepared TEA aminated UiO-66 porous material has an adsorption capacity of low-concentration hydrogen sulfide reaching 2.79mmol/g under normal temperature and pressure. It has good thermal stability, acid resistance and high selectivity, and significantly improves the dynamic desulfurization capability. Suitable for hydrogen sulfide control.
Smart Images

Figure CN118807702A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal organic framework materials, and in particular to a preparation method and application of a TEA aminated UiO-66 porous material. Background Art
[0002] Hydrogen sulfide (H2S), as a flammable and highly toxic acidic gas, is widely derived from production processes such as natural gas purification, coal gas production, and petroleum refining. As one of the main pollutants in the atmosphere, the presence of hydrogen sulfide will not only damage the environment, but also seriously corrode pipelines and equipment, directly causing economic losses. Therefore, more and more people are beginning to pay attention to hydrogen sulfide control. Hydrogen sulfide control refers to the use of absorption, adsorption, and catalytic oxidation methods to recover, utilize, or harmlessly treat hydrogen sulfide. In addition, hydrogen sulfide is also an important chemical raw material. It can be used to synthesize phosphors, photoconductors, reducing agents, and various sulfides, and can also be used in metal refining, medicine, pesticides, catalyst regeneration, etc. Therefore, as an adsorption method that can capture, store, and accumulate hydrogen sulfide, it is more suitable for hydrogen sulfide control with the advantages of low energy and high efficiency, green and pollution-free, low cost, and easy operation.
[0003] At present, the commonly used adsorbents for hydrogen sulfide treatment include activated carbon, metal oxides, molecular sieves and metal organic frameworks. Among them, metal organic frameworks (MOFs) are considered to be a material with great potential in gas adsorption. MOFs are porous skeleton structures composed of metal ions and organic linkers, with the advantages of large specific surface area, high porosity and easy modification. Compared with conventional adsorbents, MOFs have higher adsorption efficiency, but most MOFs are not stable enough, and pore collapse occurs during the adsorption of hydrogen sulfide. As a highly toxic and corrosive gas, the presence of extremely low concentrations of hydrogen sulfide will cause great harm to production and life. For the removal of low-concentration H2S content, the key is to solve the problem of insufficient adsorbent activity and improve adsorption kinetics to achieve the goal of deep desulfurization. Therefore, how to solve the pore collapse phenomenon caused by insufficient stability of MOFs during the adsorption of hydrogen sulfide, as well as the problem of insufficient adsorbent activity during the removal of low-concentration H2S content are problems that technicians in this field need to solve urgently. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a TEA-aminated UiO-66 porous material and its application, so as to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is to provide a method for preparing a TEA-aminated UiO-66 porous material, the steps comprising:
[0007] Dissolving zirconium tetrachloride, terephthalic acid and acetic acid in N,N-dimethylformamide (DMF), mixing them evenly and performing a hydrothermal reaction, and filtering, washing and drying to obtain a white solid powder;
[0008] The white solid powder is activated and added into a mixed solution of triethanolamine (TEA) and methanol. After stirring and mixing, the solid product is collected, washed and dried to obtain the TEA aminated UiO-66 porous material.
[0009] Furthermore, the mass / volume ratio of the zirconium tetrachloride, terephthalic acid, acetic acid and N,N-dimethylformamide is 2.1 g:1.5 g:7.5 mL:50 mL.
[0010] Furthermore, the temperature of the hydrothermal reaction is 120° C. and the time is 24 hours.
[0011] Furthermore, the washing is performed at least once using DMF.
[0012] Furthermore, the drying temperature is 100° C. and the drying time is 6 hours.
[0013] Furthermore, the mass volume ratio of TEA, methanol and white solid powder is 1g:20mL:4g.
[0014] Furthermore, the activation is carried out under vacuum conditions at 80° C. for 24 hours.
[0015] Furthermore, the stirring time is 12 hours.
[0016] Furthermore, the flushing is performed at least once using ethanol.
[0017] Furthermore, the drying temperature is 100° C. and the drying time is 6 hours.
[0018] The second technical solution of the present invention is to provide a TEA aminated UiO-66 porous material prepared by the above method.
[0019] The third technical solution of the present invention is to provide an application of the above-mentioned TEA aminated UiO-66 porous material as an adsorbent in hydrogen sulfide adsorption.
[0020] The present invention discloses the following technical effects:
[0021] The UiO-66 prepared by the present invention has good moisture stability, thermal stability, acid gas resistance, high selectivity, high adsorption capacity and low-cost regeneration, and introduces amino functional groups to enhance the interaction between the adsorbent and the adsorbate to improve the activity, so that the TEA aminated UiO-66 porous material (UiO-66-T product) obtained by the impregnation method can adsorb low-concentration hydrogen sulfide in an amount of up to 2.79 mmol / g under normal temperature and pressure conditions, has good mass transfer kinetics efficiency and dynamic desulfurization ability, and can be used as a potential adsorbent material for hydrogen sulfide treatment.
[0022] The preparation method of the invention is easy to operate, has a simple process, uses cheap and readily available raw materials, can be produced in large quantities, and is suitable for practical application in industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 It is a process flow chart of a specific implementation scheme of the present invention, wherein Ⅰ is a process flow chart and Ⅱ is a principle diagram;
[0025] Figure 2 The XRD patterns of the products prepared in Example 1 and Comparative Example 1 are as follows;
[0026] Figure 3 FTIR images of the products prepared in Example 1 and Comparative Example 1;
[0027] Figure 4 The SEM images of the products prepared in Example 1 and Comparative Example 1, wherein (a) is UiO-66 and (b) is UiO-66-T;
[0028] Figure 5 The breakthrough curves of the products prepared in Example 1 and Comparative Example 1 after fixed bed adsorption experiments;
[0029] Figure 6 The H2S adsorption capacity results of the products prepared for Example 1 and Comparative Example 1 at the breakthrough point, semi-dry point and dry point. DETAILED DESCRIPTION
[0030] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0031] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0032] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0033] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0034] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0035] Unless otherwise specified, the room temperature and normal temperature referred to in the specific embodiments of the present invention refer to 20-30°C.
[0036] Figure 1 It is a process flow chart of a specific implementation scheme of the present invention, wherein Ⅰ is a process flow chart and Ⅱ is a principle diagram.
[0037] Example 1
[0038] The preparation steps of TEA-aminated UiO-66 porous material are as follows:
[0039] S1, weigh 2.1 g of zirconium tetrachloride and 1.5 g of terephthalic acid, dissolve them in 50 mL of N,N-dimethylformamide (DMF) together with 7.5 mL of acetic acid at room temperature, and stir for 30 minutes to obtain a mixed solution;
[0040] S2, the mixed solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene of specification 100 mL, placed in an oven at a constant temperature of 120° C. for 24 hours to carry out a hydrothermal reaction, and the solid product was collected by filtration after cooling, washed at least once with DMF, and dried at 100° C. for 6 hours to obtain a white solid powder;
[0041] S3, activating 4 g of white solid powder under vacuum conditions at 80° C. for 24 h to obtain an activated white solid powder;
[0042] S4. Add 1 g of TEA to 20 mL of methanol, add the activated white solid powder in step S3 at 40°C, continue stirring for 12 hours, collect the solid product, rinse with anhydrous ethanol at least once, and dry at 100°C for 6 hours to obtain the TEA aminated UiO-66 porous material, recorded as UiO-66-T.
[0043] Comparative Example 1
[0044] Preparation of UiO-66 porous materials.
[0045] S1, weigh 2.1 g of zirconium tetrachloride and 1.5 g of terephthalic acid, dissolve them in 50 mL of N,N-dimethylformamide (DMF) together with 7.5 mL of acetic acid at room temperature, and stir for 30 minutes to obtain a mixed solution;
[0046] S2. The mixed solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene of 100 mL, placed in an oven at a constant temperature of 120° C. for 24 hours for hydrothermal reaction, and the solid product was collected by filtration after cooling. After washing with DMF at least once, it was dried at 100° C. for 6 hours to obtain a white solid powder, recorded as UiO-66.
[0047] Comparative Example 2
[0048] The preparation steps of modified UiO-66 porous material are:
[0049] S1, weigh 2.1 g of zirconium tetrachloride and 1.5 g of terephthalic acid, dissolve them in 50 mL of N,N-dimethylformamide (DMF) together with 7.5 mL of acetic acid at room temperature, and stir for 30 minutes to obtain a mixed solution;
[0050] S2, the mixed solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene of specification 100 mL, placed in an oven at a constant temperature of 120° C. for 24 hours to carry out a hydrothermal reaction, and the solid product was collected by filtration after cooling, washed at least once with DMF, and dried at 100° C. for 6 hours to obtain a white solid powder;
[0051] S4. Add 1 g of TEA to 20 mL of methanol, add 4 g of activated white solid powder at 40°C, continue stirring for 12 h, collect the solid product, rinse with anhydrous ethanol at least once, and dry at 100°C for 6 hours to obtain the modified UiO-66 porous material.
[0052] Test example
[0053] In order to determine the dispersion state and structure of the crystallinity of the material, the UiO-66-T prepared in Example 1 and the UiO-66 prepared in Comparative Example 1 were subjected to phase analysis by X-ray diffractometer. The specific implementation was as follows: the material was ground and placed on a cover glass for pressing and testing. The operating conditions were Cu Kα radiation, scanning range: 2θ = 5°-80°, scanning speed: 5° / min. The results are shown in FIG. Figure 2 shown.
[0054] Figure 2 The XRD patterns of the products prepared in Example 1 and Comparative Example 1 are as follows: Figure 2 It can be seen that UiO-66 exhibits standard diffraction peaks, indicating successful synthesis. The addition of TEA does not change the crystal structure of UiO-66, indicating that amines will not damage the skeleton structure of MOFs. However, the peak intensity of the material is weakened after the addition of amines, which is caused by the interaction between amines and the original UiO-66 crystals.
[0055] In order to verify the success of TEA amine functionalization, the UiO-66-T prepared in Example 1 and the UiO-66 prepared in Comparative Example 1 were subjected to infrared analysis using a Fourier transform infrared Raman spectrometer to obtain chemical structure information such as functional groups or chemical bonds of the materials. The specific implementation is as follows: the materials are dried and dehydrated, mixed with KBr and pressed into tablets, fixed in a sample cell, and infrared spectra are recorded. The wave number range is set to 4000 cm -1 -400cm -1 , resolution 4cm -1 , the results are as follows Figure 3 shown.
[0056] Figure 3 The FTIR images of the products prepared in Example 1 and Comparative Example 1 are as follows: Figure 3 It can be seen that at about 479cm -1 and 545cm -1 The peaks at 657 and 751 cm correspond to the stretching vibration of the Zr-Oμ3-OH bond and the asymmetric stretching vibration of Zr-(OC) in the Zr6 cluster. The CH and OH vibrations in H2BDC are expressed at 657 and 751 cm -1 At the same time, 1395 and 1582cm -1 The peak at 1661 cm-1 The peak at 1076 cm-1 is a carboxylic acid group, but it can be seen that the material modified with TEA amine does not have this peak. This is due to the esterification reaction between the carboxylic acid and the hydroxyl groups contained in the amine. Similarly, in the modified material, a peak different from that of UiO-66 can be seen at 1076 cm-1. -1 This is derived from the stretching vibration of the CN bond in the amine, proving that the amine group has been successfully loaded into the structure of UiO-66.
[0057] In order to observe the crystal morphology, size and size distribution of the crystal particles, the UiO-66-T prepared in Example 1 and the UiO-66 prepared in Comparative Example 1 were characterized by a scanning electron microscope. Specifically, the gold spraying treatment was performed before shooting. The results are shown in FIG. Figure 4 shown.
[0058] Figure 4 The SEM images of the products prepared in Example 1 and Comparative Example 1, wherein (a) is UiO-66 and (b) is UiO-66-T; Figure 4 It can be seen that the morphology distribution of UiO-66 is a typical octahedral configuration of MOFs materials. For UiO-66-T modified with TEA amine, it can be seen that the octahedral configuration can hardly be maintained and the surface of the material becomes rough and distorted. Generally speaking, the rougher the solid surface, the stronger its adsorption capacity.
[0059] Evaluation of the adsorption desulfurization performance of the material:
[0060] The materials prepared in Example 1 and Comparative Example 1 were used as adsorbents, and the adsorption desulfurization performance was evaluated using a fixed bed experimental device, which specifically included the following steps:
[0061] Place adsorbent (0.5g) in a fixed bed reactor, mix the same volume of silicon carbide material, and fill the reaction tube with quartz wool (3-5um) and quartz sand (40-60 mesh); then purge for 30 minutes under 100mL / min N2 atmosphere to remove impurity gases in materials and equipment; then switch to hydrogen sulfide gas with a concentration of 1000ppm, also at a flow rate of 100mL / min, and detect the change in gas concentration at the outlet at regular intervals; finally, turn off the hydrogen sulfide gas, open N2 for purging, until the outlet gas concentration is zero, and the tail gas is absorbed by the alkali solution. Among them, the hydrogen sulfide gas adsorption amount is defined as:
[0062]
[0063] In the formula, is the gas adsorption capacity of the material (mmol / g), C0 and C are the inlet and outlet gas concentrations expressed in volume (%), M is the mass of the adsorbent (g), and Q is the volume flow rate of the mixed gas (mL / min).
[0064] The gas adsorption breakthrough curve can reflect the adsorption equilibrium relationship, adsorption kinetics and mass transfer mechanism between the gas phase adsorbate and the solid phase adsorbent. In order to distinguish the adsorption capacity of the adsorbent during the adsorption process, the concepts of breakthrough point and dry point are introduced in the breakthrough curve. When the outlet concentration reaches 0.05 of the inlet concentration, the point at this time is called the breakthrough point, indicating that the gas adsorbate appears from the effluent during the adsorption process; when the outlet concentration reaches 0.95 of the inlet concentration, the point at this time is called the dry point, indicating that the adsorption capacity of the adsorbent is basically exhausted and the end point of adsorption is reached. When the outlet concentration reaches 0.5 of the inlet concentration, the point at this time is called the semi-dry point.
[0065] Figure 5 The breakthrough curves of the products prepared in Example 1 and Comparative Example 1 after fixed bed adsorption experiments are shown in Figure 1. Figure 5 It can be seen that the penetration time and mass transfer time of UiO-66-T are 45min and 191min, respectively, and the penetration time and mass transfer time of UiO-66-T are 118min and 761min, respectively. Therefore, after UiO-66 is modified with TEA amine, the penetration time and mass transfer time of the adsorbent increase to a certain extent, increasing to 1.62 times and 2.98 times of the original penetration time and mass transfer time, which indicates that the loaded amine enhances the adsorption capacity of the adsorbent for H2S.
[0066] Figure 6 The H2S adsorption capacity results of the products prepared in Example 1 and Comparative Example 1 at the breakthrough point, semi-dry point and dry point were obtained. Figure 6 It can be seen that the final adsorption capacity of UiO-66 for H2S increased from 0.89375mmol / g to 2.79375mmol / g after loading amine. TEA, as a common desulfurizer, can react with hydrogen sulfide to produce chemical adsorption force (chemical bond force), which is much stronger than the physical adsorption force (van der Waals force) generated by the raw material UiO-66 as a porous medium itself. Therefore, the H2S adsorption capacity of UiO-66-T shows a certain degree of increase compared with UiO-66. The adsorption capacity of UiO-66-T is 213% higher than that of UiO-66.
[0067] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a TEA-aminated UiO-66 porous material, characterized in that the steps include: Dissolving zirconium tetrachloride, terephthalic acid and acetic acid in N,N-dimethylformamide and mixing them evenly to carry out hydrothermal reaction, and filtering, washing and drying to obtain a white solid powder; The white solid powder is activated and added into a mixed solution of TEA and methanol. After stirring and mixing, the solid product is collected, washed and dried to obtain the TEA aminated UiO-66 porous material.
2. The preparation method according to claim 1, characterized in that: The mass / volume ratio of the zirconium tetrachloride, terephthalic acid, acetic acid and N,N-dimethylformamide is 2.1 g:1.5 g:7.5 mL:50 mL.
3. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 120° C. and the time is 24 h; the temperature of the drying is 100° C. and the time is 6 h.
4. The preparation method according to claim 1, characterized in that: The mass volume ratio of the TEA, methanol and white solid powder is 1 g:20 mL:4 g.
5. The preparation method according to claim 1, characterized in that: The activation is carried out under vacuum conditions at 80° C. for 24 hours.
6. The preparation method according to claim 1, characterized in that: The stirring time is 12h.
7. The preparation method according to claim 1, characterized in that: The drying temperature is 100° C. and the drying time is 6 hours.
8. The preparation method according to claim 1, characterized in that: The washing comprises washing with DMF at least once; and the rinsing comprises rinsing with ethanol at least once.
9. A TEA-aminated UiO-66 porous material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the TEA aminated UiO-66 porous material as claimed in claim 9 as an adsorbent in hydrogen sulfide adsorption.
Citation Information
Patent Citations
Modified UiO-66 material as well as preparation method and application thereof
CN117258766A