Gelatin-based three-dimensional block material as well as preparation method and application thereof
By introducing metal ferrocyanide into gelatin-based materials, gelatin-based three-dimensional bulk materials are prepared, which solves the problems of insufficient adsorption efficiency and radiation resistance of existing adsorbent materials in treating radioactive wastewater, and achieves efficient adsorption and ease of use. The effect of recycling.
Patent Information
- Application Number
- CN202411000508.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-22
AI Technical Summary
Existing adsorption materials have problems such as poor adsorption efficiency, poor radiation resistance, weak affinity and selectivity when treating radioactive wastewater, and the powdery materials are difficult to recycle and separate.
Gelatin is used as the base material, and metal ferrocyanide is introduced through chemical modification to prepare a gelatin-based three-dimensional bulk material, which can efficiently adsorb radionuclides such as cobalt, strontium and cesium, with fast adsorption speed, high selectivity and radiation resistance. It is characterized by high stability and the materials are easy to recycle and separate.
It achieves efficient adsorption of radionuclides such as cobalt, strontium and cesium, solves the problems of insufficient adsorption efficiency and radiation resistance of traditional materials, and simplifies the material recycling and separation process.
Smart Images

Figure CN118807709A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorption treatment of radioactive wastewater, and more specifically relates to a gelatin-based three-dimensional block material and a preparation method and application thereof. Background Art
[0002] The rapid development of nuclear energy has improved the world's energy structure and reduced greenhouse gas emissions, but it has also caused a series of pollution. The world's nuclear wastewater mainly comes from nuclear reaction processes such as nuclear power plants and nuclear bomb tests. These wastewaters are discharged and exposed to natural ecological environments such as water and soil. The radioactive pollutants contained therein, such as common cobalt, cesium, strontium, etc., not only show the chemical toxicity of heavy metals, but also have potential radioactive radiation risks and threats. Radioactive pollutants have a significant impact on human health. Radiation from radioactive substances can damage human tissues and organs, resulting in various radiation diseases, including dizziness, fatigue, hair loss, abnormal white blood cells, thrombocytopenia and other symptoms. Therefore, strict control of radioactive nuclides in radioactive wastewater has become a challenging but urgent need for environmental protection.
[0003] Effective methods for removing radionuclides from water bodies include ion exchange, solvent extraction, membrane separation and adsorption. Adsorption is one of the most widely used methods for removing radionuclides due to its advantages such as safety, high efficiency, economy, simplicity and rich variety of adsorbent materials. Therefore, research on adsorption methods and adsorbent design has important scientific research value and practical value. Activated carbon, zeolite, etc. are common adsorbents used to adsorb and remove radionuclides from water bodies. In recent years, a variety of new radionuclide adsorption materials have been continuously developed and utilized. Although some reports have pointed out that these adsorbents have a certain adsorption effect on radioactive wastewater, they still have various problems such as poor adsorption efficiency, poor radiation resistance, weak affinity and selectivity, and difficulty in separation and recovery. Summary of the invention
[0004] In view of the above technical problems, the present invention provides a gelatin-based three-dimensional block material, a preparation method and an application thereof, in order to provide a new composite material with high adsorption efficiency, high radiation resistance, strong affinity and selectivity for the effective treatment of radioactive wastewater.
[0005] To achieve the above objectives, in a first aspect, the present invention provides a method for preparing a gelatin-based three-dimensional bulk material, comprising the following steps:
[0006] Prepare gelatin solution: dissolve gelatin to form gelatin solution, the dissolution temperature is 40℃~60℃, the dissolution time is 40min~70min, and a gelatin solution of a certain concentration is obtained;
[0007] Preparation of a cross-linked intermediate material: adding a hexacyanoferrate solution of a certain concentration to the gelatin solution and performing a first ultrasonic treatment, adding an acid solution to adjust a first pH value, heating to a first temperature, mixing and stirring for a first time, and then adding a glutaraldehyde solution of a certain concentration to completely cross-link the hexacyanoferrate and the gelatin to obtain a cross-linked intermediate material;
[0008] Preparation of gelatin-based three-dimensional bulk material: slowly add a certain concentration of transition metal salt solution to the above mixed solution and perform a second ultrasonic treatment, add an alkaline solution to adjust the second pH value, mix and stir the reaction at a second temperature for a second time, so that the transition metal ions and the hexacyanoferrate on the cross-linked intermediate material form metal ferrocyanide, and then perform a third ultrasonic degassing treatment. After the first freezing and shaping, soak and wash with a solvent, then perform a second freezing and drying to obtain a gelatin-based three-dimensional bulk material.
[0009] Gelatin is a derivative of collagen, with a wide range of sources, harmless to the human body, good biocompatibility and biodegradability, and is a renewable biomass resource. According to the production and extraction process of gelatin, gelatin can be divided into three categories, namely, enzymatic gelatin, alkaline (type B) gelatin, and acid (type A) gelatin. Type A gelatin mainly comes from pig skin collagen, with an isoelectric point of 7 to 9, and often plays a role in dairy production. Type B gelatin is the largest commercial gelatin, and its main raw material is bovine collagen, with an isoelectric point of around 4 to 5. Specifically, the side chain of gelatin has high chemical reactivity and is rich in a variety of active groups such as amino and carboxyl groups, which can be further chemically modified on its surface. Gelatin is an amphoteric polyelectrolyte. Under acidic conditions, the amino groups on the surface of gelatin are positively charged; under alkaline conditions, a large number of carboxyl groups on the surface of gelatin are negatively charged. At the same time, various amino acids in gelatin molecules can form a variety of coordination forces with heavy metal ions, thereby effectively removing heavy metal ions, so gelatin has the ability to adsorb metal ions. However, pure gelatin has poor adsorption capacity for metal ions, so it is often necessary to chemically modify gelatin to enhance its adsorption capacity. The large number of active groups contained in gelatin molecules can provide effective sites for the chemical modification of gelatin, which is helpful for the chemical modification of gelatin. Metal ferrocyanide is a promising radionuclide adsorbent, which is composed of a cubic lattice structure, Fe 2+ and Fe 3+ The ions are arranged alternately in the corners; due to the designability of its crystal lattice, it can adsorb radionuclides such as cobalt, strontium and cesium from radioactive waste water with high performance.
[0010] Different from the prior art, the above technical solution uses gelatin as the base material, and chemically modifies it with metal ferrocyanide to prepare a gelatin-based three-dimensional bulk material. The material preparation method of the present invention is simple, fast, green and efficient, mild in conditions, and easy to recycle. The prepared gelatin-based three-dimensional bulk material effectively solves the problems of poor adsorption efficiency, poor radiation resistance, weak affinity and selectivity of traditional adsorption materials in the process of cobalt Co(II), strontium Sr(II), and cesium Cs(I). At the same time, it can solve the problem that traditional powdered adsorption materials are difficult to recycle and separate. The obtained gelatin-based three-dimensional bulk material has the advantages of fast adsorption speed, high adsorption selectivity, high radiation resistance stability, and easy separation and recovery.
[0011] In some embodiments, the gelatin is type B gelatin, and the concentration of the gelatin solution prepared with water as a solvent is 5wt% to 15wt%. The temperature is set to 40℃ to 60℃ without adjusting the pH, and the dissolution time is 40min to 70min. Type B gelatin is derived from pigskin or cowhide hydrolyzed by acid method. Compared with type A gelatin (derived from alkaline hydrolysis), in these embodiments, type B gelatin has better solubility near the isoelectric point, which makes the dissolution and cross-linking process of gelatin easier to control during the preparation process. The gelatin type B has a higher gel strength, which helps to make the prepared gelatin-based three-dimensional block material have better mechanical properties and structural stability. Too low a concentration of gelatin solution may result in insufficient strength of the prepared three-dimensional block material, while too high a concentration may make the solution too viscous, affecting the mixing and cross-linking effect. Within this concentration range, gelatin molecules can form enough cross-linking points to obtain a three-dimensional block material with stable structure and excellent performance. At the same time, when the dissolution temperature is lower than 40℃, gelatin cannot be completely dissolved in water; when the dissolution temperature is too high, the gelatin structure may be damaged. When the dissolution time is greater than 70 min or less than 40 min, the obtained gelatin solution will not achieve the expected effect in the subsequent steps. After repeated tests and comparisons, the inventors found that the gelatin solution prepared under the above conditions can achieve the expected mixing and cross-linking effects in the subsequent steps, improving the reaction efficiency.
[0012] In some embodiments of the present invention, the hexacyanoferrate is any one or more of potassium ferrocyanide, sodium ferrocyanide, copper ferrocyanide and calcium ferrocyanide. In a more preferred embodiment, the concentration of the hexacyanoferrate is 0.1 mol / L to 0.2 mol / L, and the volume ratio of the gelatin solution to the hexacyanoferrate solution is 1:1. Further preferably, the hexacyanoferrate used is potassium ferrocyanide. The use of potassium ferrocyanide is more effective, ensuring sufficient cross-linking between the hexacyanoferrate and the gelatin molecules, and the prepared gelatin-based three-dimensional bulk material has a better adsorption effect; when the concentration of the added potassium ferrocyanide solution is less than 0.1 mol / L, the adsorption performance of the gelatin-based three-dimensional bulk material cannot achieve the expected effect; and when the concentration of the added potassium ferrocyanide solution is greater than 0.2 mol / L, the cross-linking sites on the gelatin reach saturation, which is not conducive to the subsequent formation of the metal ferrocyanide being completely coated in the gelatin, which is not conducive to adsorption.
[0013] Optionally, the first pH value is 4.0-6.0, the first temperature is 40°C-60°C, the first time is 3h-5h, and the pH regulator is a sulfuric acid solution (mass concentration is 5%-15%). When the temperature is too low or the reaction time is too short, the reaction will be incomplete, and the product yield will be reduced. This temperature range is conducive to the cross-linking reaction, and it will not be too high to cause the gelatin solution to deteriorate or the hexacyanoferrate to decompose. The first time is set to 3h-5h to ensure that the cross-linking reaction is fully carried out to obtain an ideal cross-linked intermediate material.
[0014] Further optionally, the concentration of the added glutaraldehyde is 0.25wt% to 0.5wt%, the volume ratio of the gelatin solution to the glutaraldehyde solution is 10:(1-2), and the reaction time is 0.5h. Such a setting is the key to ensure the efficient cross-linking reaction. This concentration range of glutaraldehyde can provide sufficient cross-linking points without causing excessive cross-linking to affect the performance of the material. The reaction time is set to 0.5h, which is based on the kinetic characteristics of the cross-linking reaction, ensuring that effective cross-linking is completed in a short time, while avoiding the side effects that may be caused by too long a reaction time.
[0015] In some embodiments of the present invention, the transition metal salt is selected from Ni 2+ 、Co 2+ 、Zr 4+ , Fe 3+ , Cu 2+ Any one or more transition metal sulfate solutions, preferably Cu 2+ of sulfate solution.
[0016] More preferably, the concentration of the transition metal salt is 0.1 mol / L to 0.3 mol / L, and the molar ratio of the transition metal salt ion to the hexacyanoferrate is (1 to 2): (1 to 2).
[0017] When the added Cu 2+ When the concentration of sulfate solution is less than 0.1 mol / L, the adsorption performance of gelatin-based three-dimensional bulk materials cannot reach the expected effect; 2+ When the concentration of the sulfate solution is greater than 0.3 mol / L, the metal ferrocyanide formed subsequently will be stacked together, which is not conducive to adsorption. The molar ratio of transition metal salt ions to hexacyanoferrate is (1-2): (1-2) to ensure complete reaction and improve product yield.
[0018] In a more preferred embodiment, the speed of adding the transition metal salt solution is 10 mL / min to 15 mL / min, after 10 minutes of ultrasound, the pH value of the reaction system is adjusted to 8.0 to 10.0, the reaction temperature is 40°C to 60°C, and the reaction time is 6 hours to 8 hours. The pH value of the reaction system can be adjusted with a NaOH solution (mass concentration of 5 to 15%). When the speed of adding the transition metal salt solution is too slow or too fast, it will affect the coating of ferrocyanide in gelatin; when the temperature is too low or the reaction time is too short, it will lead to incomplete reaction and reduce the product yield.
[0019] Preferably, the third ultrasonic time is 2 minutes, the solvent is used for immersion washing at least twice, and the drying is to place the washed product at -60°C for vacuum drying for 48h to 60h. The specific cleaning method used for the in-situ growth of metal sub-solvent immersion washing is to use alcohol and deionized water to wash 2 to 4 times. The reaction mixture obtained by washing with the above solvent can effectively remove unreacted substances, salts, etc.
[0020] In the second aspect of the present invention, the inventor provides a gelatin-based three-dimensional bulk material, which is prepared by the preparation method described in the first aspect of the present invention. The present invention innovatively provides a gelatin-based three-dimensional bulk material, which has macroporous channels, can achieve the effect of high adsorption efficiency, and the synergistic effect of metal ferrocyanide having strong selectivity for radioactive nuclides. The obtained gelatin-based three-dimensional bulk material can adsorb radioactive nuclides such as cobalt, strontium and cesium with high performance, and has the characteristics of fast adsorption speed and radiation resistance stability.
[0021] In the third aspect of the present invention, the inventor provides an application of the gelatin-based three-dimensional block material as in the second aspect of the present invention in treating radioactive wastewater. The gelatin-based three-dimensional block material provided by the present invention is used to treat radioactive wastewater, which can achieve fast adsorption speed, high adsorption selectivity, and high radiation resistance stability, while solving the problem that traditional powdered adsorption materials are difficult to recover and separate.
[0022] The above-mentioned records related to the invention content are only an overview of the technical solution of the present application. In order to enable ordinary technicians in the field to more clearly understand the technical solution of the present application, and then implement it according to the text of the specification and the contents recorded in the drawings, and to make the above-mentioned purpose and other purposes, features and advantages of the present application easier to understand, the following is an explanation in combination with the specific implementation mode and drawings of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The drawings are only used to illustrate the principles, implementation methods, applications, characteristics and effects of the specific embodiments of the present application and other related contents, and shall not be considered as limitations of the present application.
[0024] In the drawings of the specification:
[0025] Figure 1 The following are photos of the gelatin aerogel (left) used in the present invention and the gelatin-based three-dimensional bulk material (right) prepared using the gelatin aerogel as a raw material;
[0026] Figure 2 It is an ultra-high resolution scanning electron microscope picture of a gelatin-based three-dimensional bulk material prepared from the raw materials gelatin and metal ferrocyanide used in the present invention;
[0027] Figure 3 It is the infrared spectrum of the gelatin-based three-dimensional bulk material prepared by the raw materials gelatin and metal ferrocyanide used in the present invention;
[0028] Figure 4 These are the test results of the strontium absorption effect of the gelatin-based three-dimensional block material prepared in Example 8 of the present invention in solutions with different pH values;
[0029] Figure 5 These are the test results of the cobalt absorption effect of the gelatin-based three-dimensional block material prepared in Example 8 of the present invention in solutions with different pH values;
[0030] Figure 6 This is a test of the cesium absorption effect of the gelatin-based three-dimensional block material prepared in Example 8 of the present invention in solutions with different pH values;
[0031] Figure 7 is the adsorption isotherm result (adsorption amount) of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention;
[0032] Figure 8 is the adsorption isotherm result (natural logarithm of adsorption amount) of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention;
[0033] Fig. 9 is the adsorption isotherm result (ratio of adsorbate concentration to adsorption amount) of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention;
[0034] Fig.10 is the adsorption kinetics result (adsorption amount) of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention;
[0035] Fig.11 is the adsorption kinetics result (adsorption rate) of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention;
[0036] Fig.12 is the adsorption kinetics result (the inverse of the adsorption rate) of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention;
[0037] Fig.13 It is the result of the coexisting ion adsorption influence of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention;
[0038] Fig.14 is an ultra-high resolution scanning electron microscope image of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention before and after cesium adsorption;
[0039] Fig.15 This is the infrared spectrum of the gelatin-based three-dimensional bulk material prepared in Example 8 of the present invention before and after the adsorption of cesium. DETAILED DESCRIPTION
[0040] In order to explain in detail the possible application scenarios, technical principles, specific schemes that can be implemented, and the purposes and effects that can be achieved, the following is a detailed description of the specific embodiments listed in conjunction with the accompanying drawings. The embodiments described herein are only used to more clearly illustrate the technical solutions of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0041] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.
[0042] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0043] In the description of this application, the term "and / or" is an expression used to describe the logical relationship between objects, indicating that three relationships may exist, for example, A and / or B, which means: A exists, B exists, and A and B exist at the same time. In addition, the character " / " in this article generally indicates that the objects before and after are in an "or" logical relationship.
[0044] In the present application, terms such as “first” and “second” are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship of quantity, priority or sequence between these entities or operations.
[0045] Without further limitations, in this application, the words "include", "comprises", "has" or other similar expressions used in the sentences are intended to cover non-exclusive inclusion. These expressions do not exclude the presence of additional elements in the process, method or product including the elements, so that the process, method or product including a series of elements may include not only those limited elements, but also other elements not explicitly listed, or also include elements inherent to such process, method or product.
[0046] Similar to the understanding in the Examination Guidelines, in this application, expressions such as "greater than", "less than", "exceed" and the like are understood to exclude the number itself; expressions such as "above", "below", "within" and the like are understood to include the number itself. In addition, in the description of the embodiments of this application, "multiple" means more than two (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups", "multiple times", etc., unless otherwise clearly and specifically limited.
[0047] Existing adsorbents used to treat radioactive waste liquid have defects and shortcomings such as lack of radiation resistance, weak affinity and selectivity for radioactive nuclides, and difficulty in separating and recovering powdered adsorbent materials. Therefore, it is very necessary to develop a composite material that is more suitable for the treatment of radioactive waste liquid. Gelatin is an excellent base material, and the inventors actively explored the feasibility and effectiveness of introducing metal ferrocyanide with high efficiency and specific affinity for radioactive nuclides on it to solve the above problems. At the same time, gelatin-based three-dimensional block materials have large pores that are not easily blocked, and are expected to improve the adsorption efficiency and reusability of radioactive nuclides. Based on this, the present invention provides a gelatin-based three-dimensional block material and a preparation method and use thereof. The prepared gelatin-based three-dimensional block material has the characteristics of fast adsorption speed, high adsorption selectivity, high radiation resistance stability, and reusability.
[0048] The main concept of the present invention is now explained through the following specific embodiments.
[0049] Unless otherwise specified, the reagents, instruments, equipment and assay methods used in the present invention are reagents, instruments, equipment and assay methods well known to those skilled in the art.
[0050] Example 1
[0051] A gelatin-based three-dimensional block material and its preparation method and use
[0052] First, prepare a gelatin solution. Take a certain amount of type B gelatin and add it to deionized water. Mix and stir for 60 minutes at 40°C to obtain a gelatin solution with a concentration of 15%. Add 0.15mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 15% sulfuric acid solution to adjust the pH value of the reaction system to 5, stir at 40°C to react for 4 hours, then add glutaraldehyde solution and react for 0.5 hours to obtain a mixed solution. Then, add 0.15mol / L ferrocyanide solution at a drop rate of 10mL / min to 15mL / min. 2+ The sulfate solution is added to the mixed solution, ultrasonically treated for 10 minutes, the pH value of the reaction system is adjusted to 8 with a NaOH solution with a mass concentration of 15%, and the mixture is stirred at 40°C for 6 hours. Ultrasonic degassing treatment is performed for 2 minutes, and the reaction product is frozen and formed, and then soaked and washed with alcohol and deionized water for 2 to 4 times, respectively. After washing, it is frozen again and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0053] 0.01 g of the gelatin-based three-dimensional block material prepared in Example 1 was added to 10 mL of 100 mg / L Sr(II), Co(II), and Cs(I) aqueous solutions, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 1.
[0054] Table 1 Adsorption effect of gelatin-based three-dimensional bulk materials prepared in Example 1 on Sr(II), Co(II) and Cs(I)
[0055]
[0056] Example 2
[0057] Preparation method and use of gelatin-based three-dimensional block material
[0058] First, prepare a gelatin solution. Take a certain amount of type B gelatin and add it to deionized water. Mix and stir at 50°C for 60 minutes to obtain a gelatin solution with a concentration of 15%. Add 0.15 mol / L potassium ferrocyanide to the above gelatin solution, ultrasonically treat for 10 minutes, use a 5% sulfuric acid solution to adjust the pH value of the reaction system to 4, stir at 40°C for 4 hours, and then add glutaraldehyde solution to react for 0.5 hours to obtain a mixed solution. Then, add 0.3 mol / L Cu at a drop rate of 10 mL / min to 15 mL / min. 2+ The sulfate solution is added to the mixed solution, ultrasonically treated for 10 minutes, the pH value of the reaction system is adjusted to 9 with a 5% NaOH solution, and the mixture is stirred at 50°C for 7 hours. The mixture is ultrasonically degassed for 2 minutes, and the reaction product is frozen and formed, and then washed with alcohol and deionized water for 2 to 4 times, frozen again after washing, and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0059] 0.01 g of the gelatin-based three-dimensional block material prepared in Example 1 was added to 10 mL, 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 2.
[0060] Table 2 Adsorption effect of gelatin-based three-dimensional bulk materials prepared in Example 2 on Sr(II), Co(II), and Cs(I)
[0061]
[0062] Example 3
[0063] Preparation method and use of gelatin-based three-dimensional block material
[0064] First, prepare a gelatin solution. Take a certain amount of type B gelatin and add it to deionized water. Mix and stir at 60°C for 60 minutes to obtain a gelatin solution with a concentration of 15%. Add 0.1 mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 10% sulfuric acid solution to adjust the pH value of the reaction system to 6, stir at 60°C for 4 hours, and then add glutaraldehyde solution to react for 0.5 hours to obtain a mixed solution. Then, add 0.15 mol / L Cu at a drop rate of 10mL / min to 15mL / min. 2+ The sulfate solution is added to the mixed solution, and the mixture is ultrasonically treated for 10 minutes. The pH value of the reaction system is adjusted to 10 with a 10% NaOH solution. The mixture is stirred at 60°C for 8 hours, and ultrasonic degassing is performed for 2 minutes. The reaction product is frozen and formed, and then washed with alcohol and deionized water for 2 to 4 times. After washing, it is frozen again and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0065] 0.01 g of the gelatin-based three-dimensional bulk material prepared in Example 3 was added to 10 mL and 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 3.
[0066] Table 3 Adsorption effect of gelatin-based three-dimensional bulk materials prepared in Example 3 on Sr(II), Co(II), and Cs(I)
[0067]
[0068] Example 4
[0069] A gelatin-based three-dimensional block material and its preparation method and use
[0070] First, prepare a gelatin solution. Take a certain amount of gelatin and add it to deionized water. Mix and stir for 60 minutes at 40°C to obtain a gelatin solution with a concentration of 10%. Add 0.1mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 10% sulfuric acid solution to adjust the pH value of the reaction system to 6, stir at 40°C to react for 4 hours, then add glutaraldehyde solution and react for 0.5 hours to obtain a mixed solution. Then, add 0.15mol / L Cu at a drop rate of 10mL / min to 15mL / min. 2+The sulfate solution is added to the mixed solution, ultrasonically treated for 10 minutes, the pH value of the reaction system is adjusted to 8 with a NaOH solution with a mass concentration of 10%, and the mixture is stirred at 40°C for 6 hours. Ultrasonic degassing treatment is performed for 2 minutes. After the reaction product is frozen and formed, it is soaked and washed with alcohol and deionized water for 2 to 4 times, respectively, and then frozen again after washing, and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0071] 0.01 g of the gelatin-based three-dimensional bulk material prepared in Example 4 was added to 10 mL and 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 4.
[0072] Table 4 Adsorption effect of gelatin-based three-dimensional bulk materials prepared in Example 4 on Sr(II), Co(II), and Cs(I)
[0073]
[0074] Example 5
[0075] A gelatin-based three-dimensional block material and its preparation method and use
[0076] First, prepare a gelatin solution. Take a certain amount of gelatin and add it to deionized water. Mix and stir at 50°C for 60 minutes to obtain a gelatin solution with a concentration of 10%. Add 0.15mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 5% sulfuric acid solution to adjust the pH value of the reaction system to 4, stir at 40°C for 4 hours, and then add glutaraldehyde solution to react for 0.5 hours to obtain a mixed solution. Then, add 0.15mol / L potassium ferrocyanide solution at a drop rate of 10mL / min to 15mL / min. 2+ The sulfate solution is added to the mixed solution, ultrasonically treated for 10 minutes, the pH value of the reaction system is adjusted to 9 with a 5% NaOH solution, and the mixture is stirred at 50°C for 7 hours. The mixture is ultrasonically degassed for 2 minutes, and the reaction product is frozen and formed, and then washed with alcohol and deionized water for 2 to 4 times, frozen again after washing, and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0077] 0.01 g of the gelatin-based three-dimensional bulk material prepared in Example 5 was added to 10 mL and 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 5.
[0078] Table 5 Adsorption effect of gelatin-based three-dimensional bulk materials prepared in Example 5 on Sr(II), Co(II), and Cs(I)
[0079]
[0080]
[0081] Example 6
[0082] A gelatin-based three-dimensional block material and its preparation method and use
[0083] First, prepare a gelatin solution. Take a certain amount of gelatin and add it to deionized water. Mix and stir at 60°C for 60 minutes to obtain a gelatin solution with a concentration of 10%. Add 0.2 mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 5% sulfuric acid solution to adjust the pH value of the reaction system to 5, stir at 60°C for 4 hours, and then add glutaraldehyde solution to react for 0.5 hours to obtain a mixed solution. Then, add 0.3 mol / L Cu at a drop rate of 10 mL / min to 15 mL / min. 2+ The sulfate solution is added to the mixed solution, ultrasonically treated for 10 minutes, the pH value of the reaction system is adjusted to 10 with a 5% NaOH solution, and the mixture is stirred at 60°C for 8 hours. The mixture is ultrasonically degassed for 2 minutes, and the reaction product is frozen and formed, and then washed with alcohol and deionized water for 2 to 4 times, frozen again after washing, and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0084] 0.01 g of the gelatin-based three-dimensional block material prepared in Example 6 was added to 10 mL and 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 6.
[0085] Table 6 Effect of the gelatin-based three-dimensional bulk material prepared in Example 6 on Sr(II), Co(II), and Cs(I)
[0086]
[0087] Example 7
[0088] A gelatin-based three-dimensional block material and its preparation method and use
[0089] First, prepare a gelatin solution. Take a certain amount of gelatin and add it to deionized water. Mix and stir at 40°C for 60 minutes to obtain a gelatin solution with a concentration of 5%. Add 0.2 mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 15% sulfuric acid solution to adjust the pH value of the reaction system to 4, stir at 40°C for 4 hours, and then add glutaraldehyde solution to react for 0.5 hours to obtain a mixed solution. Then, add 0.3 mol / L Cu at a drop rate of 10 mL / min to 15 mL / min. 2+ The sulfate solution is added to the mixed solution, ultrasonically treated for 10 minutes, the pH value of the reaction system is adjusted to 8 with a NaOH solution with a mass concentration of 15%, and the mixture is stirred at 40°C for 6 hours. Ultrasonic degassing treatment is performed for 2 minutes, and the reaction product is frozen and formed, and then soaked and washed with alcohol and deionized water for 2 to 4 times, respectively. After washing, it is frozen again and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0090] 0.01 g of the gelatin-based three-dimensional block material prepared in Example 7 was added to 10 mL and 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 7.
[0091] Table 7 Adsorption effect of gelatin-based three-dimensional bulk materials prepared in Example 7 on Sr(II), Co(II), and Cs(I)
[0092]
[0093] Example 8
[0094] A gelatin-based three-dimensional block material and its preparation method and use
[0095] First, prepare a gelatin solution. Take a certain amount of gelatin and add it to deionized water. Mix and stir at 50°C for 60 minutes to obtain a gelatin solution with a concentration of 5%. Add 0.1mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 15% sulfuric acid solution to adjust the pH value of the reaction system to 5, stir at 50°C for 4 hours, and then add glutaraldehyde solution to react for 0.5 hours to obtain a mixed solution. Then, add 0.15mol / L ferrocyanide solution at a drop rate of 10mL / min to 15mL / min. 2+The sulfate solution is added to the mixed solution, ultrasonically treated for 10 minutes, the pH value of the reaction system is adjusted to 9 with a NaOH solution with a mass concentration of 15%, and the mixture is stirred at 50°C for 7 hours. Ultrasonic degassing treatment is performed for 2 minutes, and the reaction product is frozen and formed, and then soaked and washed with alcohol and deionized water for 2 to 4 times, respectively. After washing, it is frozen again and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0096] 0.01 g of the gelatin-based three-dimensional block material prepared in Example 8 was added to 10 mL and 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 8.
[0097] Table 8 Adsorption effect of gelatin-based three-dimensional bulk materials prepared in Example 8 on Sr(II), Co(II), and Cs(I)
[0098]
[0099]
[0100] Example 9
[0101] A gelatin-based three-dimensional block material and its preparation method and use
[0102] First, prepare a gelatin solution. Take a certain amount of gelatin and add it to deionized water. Mix and stir at 60°C for 60 minutes to obtain a gelatin solution with a concentration of 5%. Add 0.15mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 10% sulfuric acid solution to adjust the pH value of the reaction system to 6, stir at 60°C for 4 hours, and then add glutaraldehyde solution to react for 0.5 hours to obtain a mixed solution. Then, add 0.15mol / L potassium ferrocyanide solution at a drop rate of 10mL / min to 15mL / min. 2+ The sulfate solution is added to the mixed solution, and the mixture is ultrasonically treated for 10 minutes. The pH value of the reaction system is adjusted to 10 using a 10% NaOH solution. The mixture is stirred at 40°C for 8 hours, and ultrasonic degassing is performed for 2 minutes. The reaction product is frozen and formed, and then washed with alcohol and deionized water for 2 to 4 times, respectively. After washing, it is frozen again and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0103] 0.01 g of the gelatin-based three-dimensional block material prepared in Example 9 was added to 10 mL and 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 hours at 25°C and an oscillation speed of 200 rpm. The results are shown in Table 9.
[0104] Table 9 Adsorption effect of gelatin-based three-dimensional bulk materials prepared in Example 9 on Sr(II), Co(II), and Cs(I)
[0105]
[0106] Example 10
[0107] A gelatin-based three-dimensional block material and preparation method thereof
[0108] First, prepare a gelatin solution. Take a certain amount of type B gelatin and add it to deionized water. Mix and stir at 50°C for 60 minutes to obtain a gelatin solution with a concentration of 5%. Add 0.1 mol / L potassium ferrocyanide solution to the above gelatin solution, ultrasonically treat for 10 minutes, use a 5% sulfuric acid solution to adjust the pH value of the reaction system to 5, stir at 50°C for 4 hours, and then add glutaraldehyde solution to react for 0.5 hours to obtain a mixed solution. Then, add 0.15 mol / L Cu at a drop rate of 10 mL / min to 15 mL / min. 2+ The sulfate solution is added to the mixed solution, and the mixture is ultrasonically treated for 10 minutes. The pH value of the reaction system is adjusted to 9 using a 5% NaOH solution. The mixture is stirred at 50°C for 7 hours, and ultrasonic degassing is performed for 2 minutes. The reaction product is frozen and formed, and then washed with alcohol and deionized water for 2 to 4 times, respectively. After washing, it is frozen again and vacuum dried at -60°C for 48 to 60 hours to obtain a gelatin-based three-dimensional block material.
[0109] See also Figure 1 From the photograph of the type B gelatin aerogel used in the present invention and the photograph of the gelatin-based three-dimensional block material prepared in Example 10, it can be seen that the prepared gelatin-based three-dimensional block material has turned red in color compared to the gelatin raw material, and the overall shape has become more fluffy.
[0110] See also Figure 2 The morphology of the type B gelatin aerogel used in the present invention and the gelatin-based three-dimensional bulk material prepared in Example 10 were observed using an ultra-high resolution scanning electron microscope, where "GA" represents gelatin aerogel, "KCuFC" represents metal ferrocyanide, and "KCuFC / GA" represents the gelatin-based three-dimensional bulk material prepared in the present invention. Figure 2The results show that both gelatin aerogel and gelatin-based three-dimensional bulk materials present a clear porous structure. This is because the water in gelatin aerogel and gelatin-based three-dimensional bulk materials is removed by sublimation during freeze drying, and the structure will not collapse, so that the original structure is preserved. After the introduction of metal ferrocyanide, the surface of the gelatin-based three-dimensional bulk material is rougher than that of the original gelatin aerogel.
[0111] See also Figure 3 The infrared spectra of the type B gelatin aerogel used in the present invention and the gelatin-based three-dimensional bulk material prepared in Example 10, respectively, detected by an infrared spectrometer, show that compared with the gelatin raw material used, the FTIR spectrum of the gelatin-based three-dimensional bulk material prepared in Example 10 is 2101 cm -1 、592cm -1 and 488cm -1 The unique peaks at represent the stretching vibration peaks of C≡N, Fe-CN and Cu-CN, respectively, indicating that the metal ferrocyanide is successfully encapsulated in gelatin, which confirms the successful synthesis of gelatin-based three-dimensional bulk materials.
[0112] Embodiment 11
[0113] Effect of pH value of radioactive waste liquid on adsorption experiment
[0114] 0.01 g of the gelatin-based three-dimensional bulk material sample prepared in Example 8 was added to 10 mL and 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I) at different pH values (pH value is 2-11), respectively, and adsorbed for 24 h at 25°C and an oscillation speed of 200 rpm. The results are as follows: Figure 4 (Sr(II)), Figure 5 (Co(II)) and Figure 6 (Cs(I)) is shown by Figure 4 , Figure 5 The results shown in Figure 2 show that the optimal pH value for adsorption of Sr(II) and Co(II) is 7. Figure 6 The results show that it has good acid-base stability and high adsorption capacity in the pH range of 2 to 11, and is suitable for removing Cs from various water bodies. + .
[0115] Example 12 Adsorption isotherm experiment
[0116] 0.01 g of the gelatin-based three-dimensional bulk material prepared in Example 8 was added to 20 mL of 0-250 mg / L aqueous solution of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 h at 25-45° C. and 200 rpm. The results are as follows: Figure 7 , Figure 8 , Fig. 9 As shown in Table 10, calculated by the Langmuir model, the maximum adsorption capacity of gelatin-based three-dimensional bulk materials for Sr(II), Co(II), and Cs(I) are 85.9 mg / g, 105.67 mg / g, and 222.22 mg / g, respectively.
[0117] Table 10 Langmuir and Freundlich parameters of gelatin-based three-dimensional bulk materials for adsorption of Sr(II), Co(II), and Cs(I)
[0118]
[0119] Example 13 Adsorption kinetics experiment
[0120] 0.01 g of the gelatin-based three-dimensional bulk material sample prepared in Example 8 was added to 10 mL, 100 mg / L aqueous solutions of Sr(II), Co(II), and Cs(I), respectively, and adsorbed for 24 h at 25°C and an oscillation speed of 200 rpm. The results are as follows: Fig.10 , Fig.11 , Fig.12 As shown in Table 11, it can be found that the gelatin-based three-dimensional bulk material can reach adsorption equilibrium in 90 min, 80 min, and 60 min, respectively.
[0121] Table 11 Kinetic fitting parameters of adsorption of Sr(II), Co(II) and Cs(I) by gelatin-based three-dimensional bulk materials
[0122]
[0123]
[0124] Embodiment 14
[0125] Effect of coexisting ions
[0126] 0.01 g of the gelatin-based three-dimensional bulk material sample prepared in Example 8 was added to 10 mL of a 100 mg / L aqueous solution, to which coexisting ions (Cs + , K + 、Na + Mg 2+ and Ca 2+ ), adsorbed for 24 h at 25 °C and 200 rpm. Fig.13 As shown, as the ion concentration increases from 0 to 400 mg / L, Na + Mg 2 + , Ca 2+With Cs + When coexisting, Cs + The adsorption capacity of K was slightly affected, and the extraction rate was greater than 90%. + The weakening effect on the adsorption capacity of gelatin-based three-dimensional bulk materials is more obvious, which is attributed to the K + Can bind to active sites on gelatin-based three-dimensional bulk materials, and The hydration radius of is similar to that of metal ferrocyanide, which matches the cavity of Therefore, in K + When the concentration is up to 400 mg / L, it has a slight effect on the adsorption of gelatin-based three-dimensional bulk materials, reducing their adsorption capacity by 16%, but it has no effect on the adsorption when the concentration is less than 400 mg / L.
[0127] Embodiment 15
[0128] See also Fig.14 The adsorption of Cs on the prepared gelatin-based three-dimensional bulk material was observed using ultra-high resolution scanning electron microscopy. + The morphology before and after the results show that the gelatin-based three-dimensional bulk material adsorbs Cs + The morphology after the reaction was almost unchanged, and the porous structure did not collapse.
[0129] Fourier transform infrared spectroscopy (FTIR) was used to characterize the adsorption of Cs on gelatin-based three-dimensional bulk materials. + Before and after testing and analysis (FTIR test results see Fig.15 ), the results showed that the adsorption of Cs + After that, the absorption peaks belonging to C≡N, Fe-CN and Cu-CN in the gelatin-based three-dimensional bulk material remained almost unchanged, indicating that [Fe(CN)6] 4- In addition, the -OH stretching vibration absorption peak in the carboxyl group changes from 3302 cm -1 Blue shift to 3316cm -1 , which means that -COOH and Cs + An interaction occurred.
[0130] Finally, it should be noted that although the above embodiments have been described in the specification and drawings of this application, this does not limit the scope of patent protection of this application. All technical solutions generated by replacing or modifying equivalent structures or equivalent processes based on the essential concept of this application using the contents recorded in the specification and drawings of this application, as well as directly or indirectly implementing the technical solutions of the above embodiments in other related technical fields, are included in the scope of patent protection of this application.
Claims
1. A method for preparing a gelatin-based three-dimensional bulk material, It is characterized in that The steps include: Prepare gelatin solution: dissolve gelatin to form gelatin solution, the dissolution temperature is 40℃~60℃, the dissolution time is 40min~70min, and a gelatin solution of a certain concentration is obtained; Preparation of a cross-linked intermediate material: adding a hexacyanoferrate solution of a certain concentration to the gelatin solution and performing a first ultrasonic treatment, adding an acid solution to adjust a first pH value, heating to a first temperature, mixing and stirring for a first time, and then adding a glutaraldehyde solution of a certain concentration to completely cross-link the hexacyanoferrate and the gelatin to obtain a cross-linked intermediate material; Preparation of gelatin-based three-dimensional bulk material: slowly add a certain concentration of transition metal salt solution to the above mixed solution and perform a second ultrasonic treatment, add an alkaline solution to adjust the second pH value, mix and stir the reaction at a second temperature for a second time, so that the transition metal ions and the hexacyanoferrate on the cross-linked intermediate material form metal ferrocyanide, and then perform a third ultrasonic degassing treatment. After the first freezing and shaping, soak and wash with a solvent, then perform a second freezing and drying to obtain a gelatin-based three-dimensional bulk material.
2. The preparation method according to claim 1, It is characterized in that In the step of preparing the gelatin solution, the gelatin is type B gelatin, and the concentration of the gelatin solution is 5wt% to 15wt%.
3. The preparation method according to claim 1, It is characterized in that The hexacyanoferrate is any one or more of potassium ferrocyanide, sodium ferrocyanide, copper ferrocyanide and calcium ferrocyanide.
4. The preparation method according to claim 1, It is characterized in that In the step of preparing the cross-linked intermediate material, the concentration of the hexacyanoferrate is 0.1 mol / L to 0.2 mol / L, and the volume ratio of the gelatin solution to the hexacyanoferrate solution is 1:
1. Optionally, the first pH value is 4.0-6.0, the first temperature is 40° C.-60° C., and the first time is 3 h-5 h. Optionally, the concentration of the glutaraldehyde solution is 0.25wt% to 0.5wt%, the volume ratio of the gelatin solution to the glutaraldehyde solution is 10:(1-2), and the reaction time is 0.5h.
5. The preparation method according to claim 1, It is characterized in that The transition metal salt is selected from Ni 2+ 、Co 2+ 、Zr 4 + , Fe 3+ , Cu 2+ Any one or more transition metal sulfates.
6. The preparation method according to claim 1, It is characterized in that The concentration of the transition metal salt is 0.1 mol / L to 0.3 mol / L, and the molar ratio of the transition metal salt ion to the hexacyanoferrate is (1 to 2): (1 to 2).
7. The preparation method according to claim 1, It is characterized in that The transition metal salt solution is added dropwise at a speed of 10 mL / min to 15 mL / min. After ultrasonication for 10 minutes, the pH value of the reaction system is adjusted to 8.0 to 10.0, the reaction temperature is 40° C. to 60° C., and the reaction time is 6 h to 8 h.
8. The preparation method according to claim 1, It is characterized in that The third ultrasonic time is 2 minutes, and the product is washed by immersion in a solvent for at least two times. The drying step is to place the washed product under vacuum drying at -60°C for 48 to 60 hours.
9. A gelatin-based three-dimensional bulk material, It is characterized in that The preparation method is described in any one of claims 1 to 8.
10. Use of the gelatin-based three-dimensional block material as claimed in claim 9 in treating radioactive wastewater.
Citation Information
Patent Citations
Gelatin composite adsorbent based technology for high efficiently removing heavy metals in water
CN106944017A
Cesium adsorption material with collagen fiber loaded Prussian blue compound as well as preparation method and application of cesium adsorption material
CN114749157A
Fluorenone polymer skin fiber membrane composite material as well as preparation method and application thereof
CN117753384A
Method for manufacturing radioactive cesium adsorptive fabric
JP2017096967A
Absorbent / hydrogel, manufacturing method for the same, and removing method for radioactive substance in using the absorbent / hydrogel
KR1020150050251A