Modified Zr-MOF material for catalyzing conversion of carbon dioxide and preparation method of modified Zr-MOF material

By introducing Ce metal into the Zr-MOF material and adjusting the organic ligand structure, a Zr-Ce-MOF material with high catalytic activity and reusability is prepared, which solves the problem of insufficient catalytic activity in the existing technology and improves the efficiency of the Zr-MOF material. The yield and production efficiency of CO2 conversion into DMC.

CN118807844APending Publication Date: 2024-10-22YANSHAN UNIV

Patent Information

Application Number
CN202410818680.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing Zr-MOF material has low catalytic activity when catalyzing the conversion of CO2 into DMC, and its reusability is limited, resulting in low DMC yield.

Method used

By introducing Ce metal precursor and adjusting the carbon chain structure, number of coordination groups and modified functional groups of organic ligands, Zr-Ce-MOF materials were prepared using a solvothermal method to enhance their catalytic performance.

Benefits of technology

It improves the catalytic activity and reusability of the Zr-Ce-MOF material, significantly increases the output of DMC, and simplifies the preparation process, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807844A_ABST
    Figure CN118807844A_ABST
Patent Text Reader

Abstract

The invention discloses a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof.The modified Zr-MOF material comprises a Ce-containing metal precursor, a Zr-containing metal precursor and an organic ligand.The preparation method comprises the steps that the Ce-containing metal precursor and the organic ligand are mixed firstly, then the Zr-containing metal precursor is doped, and the Zr-Ce-MOF material is prepared through a solvothermal method; the molar ratio of the Ce-containing metal precursor to the Zr-containing metal precursor to the organic ligand is 1: 1: 1; the organic ligand is one or more of terephthalic acid, fumaric acid, trimesic acid and 2-bromoterephthalic acid. According to the modified Zr-MOF material for catalyzing conversion of carbon dioxide and the preparation method of the modified Zr-MOF material, the preparation method is simple, the Zr-Ce-MOF material derives abundant acidic sites, the catalytic activity on DMC synthesized by CO2 and the number of repeated use times are further increased, and then the DMC yield is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst materials, and in particular to a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof. Background Art

[0002] As a cheap and readily available C1 resource, CO2 can be converted into a variety of high-value products, including urea, salicylic acid, methanol, carbonates, etc. Among them, the route of direct synthesis of dimethyl carbonate (DMC) from CO2 has attracted the attention of more and more researchers. This route uses CO2 and methanol to synthesize DMC through a one-step reaction under appropriate conditions. The only by-product is water, and the atomic utilization rate is high. Moreover, in the whole process, the raw materials are cheap and readily available, and all the materials involved are non-toxic, especially the use of CO2, a greenhouse gas, which is very friendly to the environment.

[0003] However, the current DMC yield of this route is low. This is mainly due to two aspects: first, CO2 is very stable and requires a lot of energy to activate; second, the Gibbs free energy of the reaction △G 298k =26.2 kJ / mol>0, which means that the reaction is subject to thermodynamic limitations, and the limitations on the reaction equilibrium can be eliminated by increasing the CO2 pressure or removing the by-product H2O in a timely manner.

[0004] Compared with the industrialized route, the direct synthesis of DMC from DMC and methanol has the advantages of simple process, high atomic utilization, only H2O as a by-product, green and environmentally friendly process. This route is of great significance for CO2 emission reduction.

[0005] In recent years, metal organic frameworks (MOFs) are organic-inorganic hybrid materials with intramolecular pores formed by self-assembly of organic ligands and metal ions or clusters through coordination bonds. Due to their adjustable structure and large specific surface area, they have begun to be used for resource utilization of CO2. When MOFs are used for CO2 conversion, their abundant Lewis acid sites mainly adsorb and activate CO2. These acid sites can act as active sites to activate CO2 and methanol, especially to activate methanol to generate methoxy groups, which are important intermediates for the formation of DMC.

[0006] In the existing technology, Zr-MOF material has good water resistance and thermal stability, and is one of the most stable materials among MOFs materials. In addition to excellent stability, Zr-MOF has abundant acidic sites derived from Zr metal. However, when Zr-MOF is used to catalyze CO2 conversion, it has defects such as low catalytic activity and limited number of reusable times, resulting in low DMC production. Summary of the invention

[0007] The purpose of the present invention is to provide a modified Zr-MOF material for catalyzing the conversion of carbon dioxide and a preparation method thereof. The preparation method is simple, and the Zr-Ce-MOF material derives abundant acidic sites, which further improves the catalytic activity of CO2 to synthesize DMC and the number of times it can be reused, thereby increasing the DMC yield.

[0008] To achieve the above object, the present invention provides a modified Zr-MOF material for catalyzing carbon dioxide conversion, comprising a Ce-containing metal precursor, a Zr-containing metal precursor and an organic ligand, wherein the Ce-containing metal precursor and the organic ligand are first mixed, and then the Zr-containing metal precursor is doped to obtain a Zr-Ce-MOF material by a solvothermal method;

[0009] The molar ratio of the Ce-containing metal precursor, the Zr-containing metal precursor and the organic ligand is 1:1:1;

[0010] The organic ligand is one or more of terephthalic acid, fumaric acid, trimesic acid and 2-bromoterephthalic acid.

[0011] To achieve the above object, the present invention also provides a method for preparing a modified Zr-MOF material for catalyzing carbon dioxide conversion, comprising the following steps:

[0012] S1, adding a Ce-containing metal precursor and an organic ligand into an N,N-dimethylformamide solution in proportion and stirring for 30 minutes to obtain a mixed solution A;

[0013] S2, dissolving the Zr-containing metal precursor in N,N-dimethylformamide solution according to the proportion and stirring for 30 minutes to obtain a mixed solution B;

[0014] S3. Under vigorous stirring, the mixed solution B obtained in the above step S2 is added dropwise to the mixed solution A obtained in the above step S1 and stirred for 30 minutes, and the Zr-Ce-MOF material is prepared by a solvothermal method.

[0015] Preferably, in step S1, the Ce-containing metal precursor is (NH4)2Ce(NO3)6.

[0016] Preferably, in step S2, the Zr-containing metal precursor is ZrCl4.

[0017] Preferably, in step S3, the Zr-Ce-MOF material is prepared by a solvothermal method, and the specific process is as follows:

[0018] The mixed liquid was loaded into a hydrothermal kettle and placed in an oven preheated to 120°C for 24 hours. After the hydrothermal kettle was cooled to room temperature, the mixture was taken out and centrifuged to obtain a white precipitate at the lower layer. The precipitate was centrifuged and washed several times with N,N-dimethylformamide solution and acetone, and then dried in a 70°C forced air drying oven for 4 hours to obtain Zr-Ce-MOF material.

[0019] Therefore, the present invention adopts the above-mentioned modified Zr-MOF material for catalyzing carbon dioxide conversion and its preparation method, which has the following technical effects:

[0020] (1) The present invention adopts a solvent thermal method, the preparation method is simple, and is suitable for large-scale production of DMC synthesized from CO2.

[0021] (2) The present invention introduces Ce metal into the Zr-MOFs material and adjusts the carbon chain structure of the organic ligand, the number of coordination groups and the type of modified functional groups. It is proved that the Zr-Ce-MOF material with the smallest spherical particles, the highest pore volume content, the best weak alkalinity, the most medium-strength acid sites and the most Lewis acid sites that can adsorb and activate methanol has the best catalytic performance.

[0022] (3) When fumaric acid is used as an organic ligand in the present invention, the carbon chain structure of fumaric acid is a short straight chain double bond structure. Compared with the benzene ring structure of terephthalic acid, it has the best crystallinity, a large amount of surface Zr content and the most Lewis acid sites that can adsorb and activate methanol, and has the best catalytic performance.

[0023] (4) When the present invention uses trimesic acid as an organic ligand and the number of coordinating groups is 2, the corresponding Zr-Ce-MOF material has a large surface Zr content, a relatively high content of Lewis base sites (Zr-O-) that can adsorb and activate CO2 and methanol, and has the best catalytic performance.

[0024] (5) When 2-bromoterephthalic acid is used as the organic ligand in the present invention, the bromine-modified functional group enables the corresponding Zr-Ce-MOF material to have a hexahedral crystal morphology, a minimum particle size, and a maximum O v The content and the largest number of Lewis acid sites that can adsorb and activate methanol have the best catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is an XRD diagram of Example 1 of a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof according to the present invention;

[0026] Figure 2 It is a N2 adsorption-desorption isotherm diagram of Example 1 of a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof of the present invention;

[0027] Figure 3 This is a TEM image of Example 1 of a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof according to the present invention;

[0028] Figure 4 TEM images of catalysts with different carbon chain structures synthesized in an embodiment of a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof according to the present invention, wherein (a) is Zr-1B-2C, (b) is Zr-2B-2C, (c) is Zr-3B-2C, (d) is Zr-1C=C-2C, and (e) is Zr-2C=C-2C;

[0029] Figure 5 It is a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof according to an embodiment of the present invention, wherein the catalysts with different carbon chain structures are synthesized in an N2 adsorption-desorption isotherm diagram;

[0030] Figure 6 This is a pore size distribution diagram of catalysts with different carbon chain structures synthesized in an embodiment of a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof of the present invention;

[0031] Figure 7 This is a Py-IR graph of a catalyst with different carbon chain structures synthesized in an embodiment of a modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof according to the present invention. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0033] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0034] Embodiment 1

[0035] A method for preparing a modified Zr-MOF material for catalyzing carbon dioxide conversion is as follows:

[0036] S1. Completely dissolve 5 mmol (NH4)2Ce(NO3)6 and 5 mmol terephthalic acid in 125 ml N,N-dimethylformamide solution (DMF) and stir for 30 min to obtain a mixed solution A.

[0037] S2. Dissolve 5 mmol ZrCl4 in 50 ml DMF and stir for 30 min to obtain a mixed solution B.

[0038] S3. Under vigorous stirring, add the mixed solution B dropwise into the mixed solution A and stir for 30 minutes. The mixed solution is charged into a hydrothermal kettle and placed in an oven preheated to 120°C for 24 hours. After the hydrothermal kettle is cooled to room temperature, the mixture is taken out and centrifuged to obtain a white precipitate in the lower layer. The precipitate is centrifuged and washed several times with N,N-dimethylformamide solution and acetone, and then dried in a 70°C forced air drying oven for 4 hours to obtain Zr-Ce-MOF (Ce is added first and then Zr) material.

[0039] Embodiment 2

[0040] The difference from Example 1 is that, in step S1, 5 mmol (NH4) 2Ce (NO3) 6 and 5 mmol fumaric acid are completely dissolved in 125 ml N, N-dimethylformamide solution (DMF) and stirred for 30 min to obtain a mixed solution A.

[0041] Embodiment 3

[0042] The difference from Example 1 is that, in step S1, 5 mmol (NH4)2Ce(NO3)6 and 5 mmol trimesic acid are completely dissolved in 125 ml N,N-dimethylformamide solution (DMF) and stirred for 30 min to obtain a mixed solution A.

[0043] Embodiment 4

[0044] The difference from Example 1 is that, in step S1, 5 mmol (NH4)2Ce(NO3)6 and 5 mmol 2-bromoterephthalic acid are completely dissolved in 125 ml N,N-dimethylformamide solution (DMF) and stirred for 30 min to obtain a mixed solution A.

[0045] Comparative Example 1

[0046] The difference from Example 1 is that organic ligands with different carbon chain structures are used, namely commercially available biphenyl dicarboxylic acid, terphenyl dicarboxylic acid, and cis-dienedioic acid.

[0047] Comparative Example 2

[0048] The difference from Example 1 is that organic ligands with different numbers of coordination groups are used, and commercially available pyromellitic acid is used.

[0049] Comparative Example 3

[0050] The difference from Example 1 is that different types of organic ligands with modified functional groups are used, including commercially available 2-aminoterephthalic acid, 2-nitroterephthalic acid and 2-hydroxyterephthalic acid.

[0051] Experimental Testing

[0052] The crystal morphology and morphology of the catalyst prepared in Example 1 were characterized by XRD, TEM and N2 isothermal adsorption-desorption.

[0053] like Figure 1 As shown, four catalysts, namely Zr-MOF, Ce-Zr-MOF (Zr was added first and then Ce was doped), Zr-Ce-MOF (Ce was added first and then Zr was added), and Ce-MOF, were characterized at the same time. As can be seen from the figure, Zr-MOF exhibits characteristic diffraction peaks corresponding to the (111), (002) and (224) crystal planes of UiO-66 at 7.5°, 8.8° and 25.9°, respectively, indicating the successful synthesis of the UiO-66 structure. After the introduction of metallic Ce, this characteristic peak in Zr-Ce-MOF moved to 7.5°, which confirmed that the Ce atoms had been successfully incorporated into the framework lattice. This crystal structure deformation caused by Ce doping may be due to the Ce 4+ and Zr 4+ The radius of Ce(Ce 3+ ) in different valence states. In addition, after the introduction of metal Ce, the diffraction peak intensity of the material increased sharply, indicating that Ce doping enhanced the crystallinity of UiO-66 material.

[0054] like Figure 3 As shown in the figure, the material is spherical in shape, which is consistent with the crystal structure shown in the XRD pattern. Figure 2 As shown in the figure, four catalysts, namely Zr-MOF, Ce-Zr-MOF (adding Zr first and then doping Ce), Zr-Ce-MOF (adding Ce first and then adding Zr), and Ce-MOF, were characterized at the same time. As can be seen from the figure, the N2 adsorption-desorption isotherm is type I, indicating that they are all microporous materials. The pore size is mainly distributed in the range of 0.5-1.0nm, which once again confirms that the material is a microporous material, indicating the successful synthesis of Zr / Ce-MOF microporous material.

[0055] The catalysts prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were used in the process of synthesizing DMC from CO2 and CH3OH. The preparation method was as follows: a specific amount of CH3OH, 2-CY, Mesi and catalyst were added to a micro-autoclave, and the mixture was purged with N2 three times to remove the air in the sealed autoclave. Finally, CO2 at a specific pressure was added to the autoclave at 900 r·min. -1 and react under specific temperature conditions.

[0056] According to the organic ligands used in Examples 1 to 4 and Comparative Examples 1 to 3, the synthesized catalysts are named as follows:

[0057] Different carbon chain structures of organic ligands: Zr-1B-2C, Zr-2B-2C, Zr-3B-2C, Zr-1C=C-2C, Zr-2C=C-2C; different numbers of coordinating groups on organic ligands: Zr-1B-2C, Zr-1B-3C, Zr-1B-4C; different functional groups introduced into organic ligands: Zr-BDC, Zr-BDC-NH2, Zr-BDC-Br, Zr-BDC-NO2, Zr-BDC-OH.

[0058] The structural formula and name of the organic ligand are as follows:

[0059]

[0060]

[0061] Among them, (a) is an organic ligand with different carbon chain structures, (b) is an organic ligand with different numbers of coordination groups, and (c) is an organic ligand with different structural formulas of modified functional groups.

[0062] Catalytic activity and structural analysis of catalysts with different carbon chain structures:

[0063] Depend on Figure 4 It can be seen that with the increase in the number of benzene rings in the organic ligand, the morphology of the Zr-based MOF evolves from a cube of about 200nm to a cuboid of 300nm in length. This is because the increase in the number of benzene rings changes the crystal agglomeration during the formation of MOF material particles. When the carbon chain structure of the organic ligand is a straight chain double bond, the particles of Zr-1C=C-2C and Zr-2C=C-2C are both cuboids of about 100-150nm, and the particle size of Zr-1C=C-2C is more uniform. This shows that the carbon chain structure of the organic ligand has an important influence on the morphology of the MOF material.

[0064] Depend on Figure 5 and Figure 6 It can be seen that the N2 adsorption isotherms of Zr-xB(C=C)-2C all show type I, indicating that they have microporous structures. Among them, Zr-2B-2C, Zr-3B-2C, and Zr-2C=C-2C have hysteresis loops, indicating that these three materials may have mesoporous structures. Among them, Zr-1B-2C shows the highest specific surface area (1159.00m 2 ·g -1 ), its pore volume (0.54m 3 ·g -1 ) and micropore volume (0.34m 3 ·g -1 ) is also the largest. As the number of benzene rings on the organic ligand increases, the specific surface area of ​​the material decreases to 148.20 m 2 ·g -1(Zr-2B-2C), 108.16m 2 ·g -1 (Zr-3B-2C). When the organic ligand is a linear double bond, the specific surface area of ​​Zr-1C=C-2C is 290.17 m 2 ·g -1 , and the specific surface area of ​​Zr-2C=C-2C drops sharply to 7.50m 2 ·g -1 Similarly, as the number of benzene rings increases, the pore volume of the material decreases to 0.13 m 3 ·g -1 (Zr-2B-2C), 0.20m 3 ·g -1 (Zr-3B-2C). When the organic ligand is a linear double bond structure, the pore volume of Zr-1C=C-2C is 0.19m 3 ·g -1 After the linear double bond grows, the pore volume of Zr-2C=C-2C drops sharply to 0.01m 3 ·g -1 . Moreover, when the number of benzene rings in the organic ligand increases from 1 to 2, the pore size distribution changes from 0.5-1nm to 45-100nm. As the number of benzene rings further increases to 3, the pore size distribution is concentrated in the range of 55-120nm. When the benzene ring in the organic ligand changes to a linear double bond structure, the pore size distribution is in the range of 0.5-1nm and 40-100nm. When the number of carbons increases, the pore size is concentrated in the range of 50-120nm.

[0065] Depend on Figure 7 It can be seen that the more acidic sites on the catalyst, the higher its catalytic activity. Methanol can be adsorbed and activated on LAS, which is a key factor in improving catalytic activity. The high intensity of the LAS characteristic peak in the Py-IR spectra of Zr-2B-2C and Zr-1C=C-2C proves this. In summary, increasing the number of benzene rings on the organic ligand or adjusting it to a linear double bond structure will increase the acidic sites of the material, thereby improving the catalytic activity of Zr-based MOF.

[0066] And fumaric acid was used as the catalyst Zr-1C=C-2C with organic ligand, and 2.78mmol DMC was obtained under the reaction conditions of 150℃, 2.6MPa and 6h, which was the highest DMC yield.

[0067] Catalytic activity and structural analysis of catalysts with different numbers of coordination groups:

[0068] The same analytical process as for catalysts with different carbon chain structures was used to demonstrate the successful synthesis of the catalyst. It was found that when the number of coordination groups in the organic ligand changed, the surface Zr content changed significantly, corresponding to the Zr-O - The characteristic peaks of the Lewis basic sites also changed significantly. The catalyst after the reaction can be observed to have intermediates such as p-CO3, i-HCO3, m-CO3, t-OCH3, b-OCH3, etc. after the Lewis basic sites are activated. Therefore, the effect of the number of coordination groups on the CO2 conversion performance is likely to come from the Zr-O - The catalyst Zr-BDC-Br with trimesic acid as the organic ligand has a large surface Zr content, a high content of Lewis basic sites (Zr-O - ).

[0069] And the catalyst Zr-1B-3C with trimesic acid as the organic ligand, under the reaction conditions of 150℃, 2.6MPa, and 6h, obtained 2.61mmol DMC, which was the highest DMC yield.

[0070] Catalytic activity and structural analysis of catalysts with different modified functional groups:

[0071] The same analytical process as catalysts with different carbon chain structures was used to demonstrate the successful synthesis of the catalyst. It was found that after the organic ligands were modified by different functional groups, the morphology of the Zr-based MOF evolved from a cube of about 200 nm to a cube or hexahedron of 80-150 nm. Among them, the catalyst Zr-BDC-Br with 2-bromoterephthalic acid as the organic ligand has a hexahedral crystal morphology, the smallest particle size, and the highest O v The content and the largest number of Lewis acid sites that can adsorb and activate methanol.

[0072] And 2-bromoterephthalic acid was used as the catalyst Zr-BDC-Br of the organic ligand, and 5.82 mmol of DMC was obtained under the reaction conditions of 150°C, 4.6 MPa, and 6 h, which was the highest DMC yield.

[0073] In summary, the catalyst with the smallest spherical particles, the highest pore volume content, the best weak alkalinity, the most moderate acid sites, and the most Lewis acid sites that can adsorb and activate methanol has the best catalytic performance.

[0074] Therefore, the present invention adopts the above-mentioned modified Zr-MOF material for catalyzing the conversion of carbon dioxide and its preparation method. The preparation method is simple, and the Zr-Ce-MOF material derives abundant acidic sites, which further improves the catalytic activity of CO2 to synthesize DMC and the number of times it can be reused, thereby increasing the DMC yield.

[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A modified Zr-MOF material for catalyzing carbon dioxide conversion, characterized in that: The method comprises a Ce-containing metal precursor, a Zr-containing metal precursor and an organic ligand, wherein the Ce-containing metal precursor and the organic ligand are first mixed, and then the Zr-containing metal precursor is doped to prepare a Zr-Ce-MOF material by a solvothermal method; The molar ratio of the Ce-containing metal precursor, the Zr-containing metal precursor and the organic ligand is 1:1:1; The organic ligand is one or more of terephthalic acid, fumaric acid, trimesic acid and 2-bromoterephthalic acid.

2. A method for preparing a modified Zr-MOF material for catalyzing carbon dioxide conversion, characterized in that: The steps include: S1, adding a Ce-containing metal precursor and an organic ligand into an N,N-dimethylformamide solution in proportion and stirring for 30 minutes to obtain a mixed solution A; S2, dissolving the Zr-containing metal precursor in N,N-dimethylformamide solution according to the proportion and stirring for 30 minutes to obtain a mixed solution B; S3. Under vigorous stirring, the mixed solution B obtained in the above step S2 is added dropwise to the mixed solution A obtained in the above step S1 and stirred for 30 minutes, and the Zr-Ce-MOF material is prepared by a solvothermal method.

3. The method for preparing a modified Zr-MOF material for catalyzing carbon dioxide conversion according to claim 2, characterized in that: In step S1, the Ce-containing metal precursor is (NH4)2Ce(NO3)6.

4. A modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof according to claim 2, characterized in that: In step S2, the Zr-containing metal precursor is ZrCl4.

5. A modified Zr-MOF material for catalyzing carbon dioxide conversion and a preparation method thereof according to claim 2, characterized in that: In step S3, the Zr-Ce-MOF material is prepared by a solvothermal method, and the specific process is as follows: The mixed liquid was loaded into a hydrothermal kettle and placed in an oven preheated to 120°C for 24 hours. After the hydrothermal kettle was cooled to room temperature, the mixture was taken out and centrifuged to obtain a white precipitate at the lower layer. The precipitate was centrifuged and washed several times with N,N-dimethylformamide solution and acetone, and then dried in a 70°C forced air drying oven for 4 hours to obtain Zr-Ce-MOF material.

Citation Information

Patent Citations

  • Preparation method for nickel / nitrogen-mixed carbon microsphere combined hydrogen evolution electrode

    CN107326395A

  • Stabilised antiseptic preparations

    EP3355860A1

Cited By

  • Cu-coated MOF-808 (Zr) catalyst as well as preparation method and application thereof

    CN122558564A