Quantitative roller coating method for oil on surface of steel plate sample

By using a smooth glass rod to rotate and contact the steel plate, the problem of manual oiling being difficult to achieve uniform quantification is solved, and the oil liquid is evenly coated on the surface of the steel plate sample, ensuring the accuracy and reliability of the experimental results at a low cost.

CN118808086APending Publication Date: 2024-10-22BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410802392.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the steel plate sample experiment, manual oiling is difficult to achieve uniformity and quantification, which affects the accuracy of the experimental results.

Method used

Use a smooth glass rod with a diameter of 0.5-1cm as a tool, absorb the oil through the buret and rotate it to fully infiltrate the central part, rotate it to contact the steel plate to achieve quantitative roller coating, measure the weight difference to calculate the oil coating amount, and adjust the roller coating cycle to ensure the target amount of oil is applied.

Benefits of technology

It achieves uniform and quantitative coating of oil on the surface of the steel plate sample, ensuring the accuracy and reliability of the experimental results, with low cost and simple operation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a quantitative roller coating method for oil on the surface of a steel plate sample, and belongs to the field of oil performance experiments and steel plate antirust experiments. The effect of uniformly coating quantitative oil samples on small-size steel plate sample sheets can be simply achieved, the cost is low, and the implementation is convenient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of oil performance experiments and steel plate anti-rust experiments, and in particular to a method for quantitatively rolling oil on the surface of a steel plate sample. Background Art

[0002] As the application scenarios of steel plates continue to expand, the demand for surface morphology and protective oils has continued to refine. The comprehensive performance of "steel plate + oil" has increasingly become the core of testing and evaluation for steel mills and oil manufacturers.

[0003] When oils with different functions, models and compositions such as anti-rust oil and rolling oil for steel plates are combined with various surface variables of steel plates such as different surface morphologies, surface treatment methods and surface compositions of steel plates, the comprehensive performance exhibited requires various tests and experiments.

[0004] However, during the experiment, unlike the large-scale oil spraying system of the steel plant production line, the steel plate samples are small in size, and it is difficult to achieve uniform and quantitative manual oiling, which seriously affects various experimental results. Therefore, the present method is specially invented. Summary of the invention

[0005] The purpose of the present invention is to provide a method for quantitatively rolling oil on the surface of a steel plate sample, so as to ensure the quantification and uniformity of manual oiling of steel plate samples, so as to ensure accurate and reliable results when relevant experiments are carried out.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for quantitatively rolling oil coating on the surface of a steel plate sample, comprising the following steps:

[0008] 1) Use a smooth glass rod with a diameter of 0.5-1cm as a tool, test the cycle of the glass rod rolling along the length of the steel plate, target the total amount of oil coated on the steel plate, and measure the weight of the glass rod when it is clean;

[0009] 2) Use a burette to absorb the oil, drip the oil on the center of the smooth glass rod while rotating the glass rod to make the center of the glass rod fully soaked in the oil, wait for 8-12 seconds until no more drops fall, and measure the weight of the oiled glass rod, so that the amount of oil on the glass rod each time is the "total target oil amount / rolling cycle" amount;

[0010] 3) Place a glass rod with oil on one end of the steel plate and rotate it to contact the steel plate. Do not reciprocate or slide during the rotation. Measure the weight of the glass rod again. The difference between the weight and the weight is the current amount of oil applied to the steel plate.

[0011] 4) Repeat steps 2) and 3) until the entire sample length area is completed. In the last cycle, control the difference from the target oil volume. If it is insufficient, increase the rolling cycle and calculate the weight difference until it meets the target;

[0012] 5) Leave the sample horizontally for a certain period of time to make it uniform.

[0013] Furthermore, in the step 2), the mixture is left to stand for 10 seconds until no liquid drops fall.

[0014] Furthermore, in step 5), the sample is left horizontally for 1 hour.

[0015] Furthermore, a smooth glass rod with a diameter of 0.5 cm was selected as a tool.

[0016] Furthermore, a smooth glass rod with a diameter of 1 cm was selected as a tool.

[0017] Compared with the prior art, the beneficial technical effects of the present invention are:

[0018] The present invention adopts a glass rod of a certain size, utilizes the surface tension and large viscosity of the oil, and can achieve the effect of uniformly coating a small-sized steel plate sample with a quantitative oil sample by dipping a quantitative oil liquid and then rolling it, which is low-cost and easy to achieve. DETAILED DESCRIPTION

[0019] Example 1

[0020] A method for quantitatively rolling oil on the surface of a steel plate sample comprises the following steps:

[0021] 1) Use a smooth glass rod with a diameter of 0.5 cm as a tool, test the cycle of the glass rod rolling along the length of the steel plate (such as: rotating 3 times), target the total amount of oil coated on the steel plate, and measure the weight of the glass rod when it is clean.

[0022] 2) Use a burette to absorb the oil, drip the oil in the center of the smooth glass rod (the length range is the same as the width of the steel plate sample) and rotate the glass rod at the same time to make the center of the glass rod fully immersed in the oil. Wait for about 10 seconds until no droplets fall, and measure the weight of the oiled glass rod so that the amount of oil on the glass rod each time is approximately "total target oil amount / rolling cycle".

[0023] 3) Place a glass rod with oil on one end of the steel plate and rotate it to make the oil on the steel plate. Do not reciprocate or slide during the rotation. Measure the weight of the glass rod again. The difference between the weight of the glass rod and the oil on the steel plate is the current amount of oil applied to the steel plate.

[0024] 4) Repeat steps 2) and 3) until the entire sample length area is completed (according to the rotation cycle tested previously, such as 3 rotations). In the last cycle, control the difference from the target oil volume. If it is insufficient, increase the rolling cycle and calculate the weight difference until it meets the target.

[0025] 5) Leave the sample horizontally for 1 hour to allow it to become homogenous.

[0026] The present invention adopts a glass rod of a certain size, utilizes the surface tension and large viscosity of the oil, and can achieve the effect of uniformly coating a small-sized steel plate sample with a quantitative oil sample by dipping a quantitative oil liquid and then rolling it, which is low-cost and easy to achieve.

[0027] Example 2

[0028] A method for quantitatively rolling oil on the surface of a steel plate sample comprises the following steps:

[0029] 1) Use a smooth glass rod with a diameter of 1 cm as a tool, test the cycle of the glass rod rolling along the length of the steel plate (such as 5 rotations), target the total amount of oil coated on the steel plate, and measure the weight of the glass rod when it is clean.

[0030] 2) Use a burette to absorb the oil, drip the oil in the center of the smooth glass rod (the length range is the same as the width of the steel plate sample) and rotate the glass rod at the same time to make the center of the glass rod fully immersed in the oil. Wait for about 12 seconds until no droplets fall, and measure the weight of the oiled glass rod so that the amount of oil on the glass rod each time is approximately "total target oil amount / rolling cycle".

[0031] 3) Place a glass rod with oil on one end of the steel plate and rotate it to make the oil on the steel plate. Do not reciprocate or slide during the rotation. Measure the weight of the glass rod again. The difference between the weight of the glass rod and the oil on the steel plate is the current amount of oil applied to the steel plate.

[0032] 4) Repeat steps 2) and 3) until the entire sample length area is completed (according to the rotation cycle tested previously, such as 5 rotations). In the last cycle, control the difference from the target oil volume. If it is insufficient, increase the rolling cycle and calculate the weight difference until it meets the target.

[0033] 5) Leave the sample horizontally for 1.5 hours to allow it to become homogenous.

[0034] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for quantitatively rolling oil on the surface of a steel plate sample, characterized in that: The steps include: 1) Use a smooth glass rod with a diameter of 0.5-1cm as a tool, test the cycle of the glass rod rolling along the length of the steel plate, target the total amount of oil coated on the steel plate, and measure the weight of the glass rod when it is clean; 2) Use a burette to absorb the oil, drip the oil on the center of the smooth glass rod while rotating the glass rod to make the center of the glass rod fully soaked in the oil, wait for 8-12 seconds until no more drops fall, and measure the weight of the oiled glass rod, so that the amount of oil on the glass rod each time is the "total target oil amount / rolling cycle" amount; 3) Place a glass rod with oil on one end of the steel plate and rotate it to contact the steel plate. Do not reciprocate or slide during the rotation. Measure the weight of the glass rod again. The difference between the weight and the weight is the current amount of oil applied to the steel plate. 4) Repeat steps 2) and 3) until the entire sample length area is completed. In the last cycle, control the difference from the target oil volume. If it is insufficient, increase the rolling cycle and calculate the weight difference until it meets the target; 5) Leave the sample horizontally for a certain period of time to make it uniform.

2. The method for quantitatively rolling oil coating on the surface of a steel plate sample according to claim 1, characterized in that: In the step 2), the mixture is left to stand for 10 seconds until no liquid drops fall.

3. The method for quantitatively rolling oil coating on the surface of a steel plate sample according to claim 1, characterized in that: In the step 5), the sample is placed horizontally for 1 hour.

4. The method for quantitatively rolling oil coating on the surface of a steel plate sample according to claim 1, characterized in that: A smooth glass rod with a diameter of 0.5 cm was used as a tool.