Continuous production method and system for copper alloy material
By coating the surface of copper alloy materials with a composite crystalline layer and using nano-carbon fibers and immersion cooling of amorphous raw materials, the problem of insufficient corrosion resistance of copper alloy materials in corrosive environments is solved, and the mechanical strength and corrosion resistance are improved. performance.
Patent Information
- Application Number
- CN202410885565.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-22
AI Technical Summary
Existing copper alloy materials have insufficient corrosion resistance in corrosive environments, especially in marine environments and acid rain areas. They are prone to rust after long-term use and have low mechanical strength.
A continuous production method of copper alloy materials is adopted. By coating the surface of the copper alloy matrix with a composite crystalline layer, nanocarbon fibers and amorphous raw materials are used to immerse and cool in organic solvents to form a composite crystalline layer to improve corrosion resistance. performance and mechanical strength.
It effectively improves the corrosion resistance and mechanical strength of copper alloy materials, especially the bending strength, and the modified carbon nanofibers are more evenly dispersed and have better stability.
Smart Images

Figure HDA0004925955470000011
Abstract
Description
Technical Field
[0001] The invention relates to the field of copper alloy materials, and in particular to a method and system for continuous production of copper alloy materials. Background Art
[0002] Copper alloy is an alloy composed of pure copper as the matrix and one or more other elements. Pure copper is purple-red and is also called red copper. The density of pure copper is 8.96 and the melting point is 1083℃. It has excellent electrical conductivity, thermal conductivity, ductility and corrosion resistance. It is mainly used to make electrical equipment such as generators, busbars, cables, switchgear, transformers, and heat exchangers, pipelines, flat-plate collectors of solar heating devices and other heat-conducting equipment.
[0003] However, its corrosion resistance becomes particularly important when it is used for a long time and exposed to corrosive environments, such as marine environments and acid rain areas, so it needs to be improved in this regard. Summary of the invention
[0004] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a continuous production system and method for copper alloy materials.
[0005] The technical solution of the present invention is as follows:
[0006] A continuous production method of copper alloy material, comprising raw material pretreatment, smelting and continuous casting and cladding;
[0007] Wherein, the continuous casting coating is to coat the surface of the copper alloy substrate obtained after smelting with a composite crystalline layer;
[0008] The preparation method of the composite crystalline layer is as follows:
[0009] S1: dispersing carbon nanofibers in an organic solvent to obtain a pretreatment solution;
[0010] S2: melting the amorphous raw material to obtain a melt;
[0011] S3: Immersing the copper alloy substrate in the pretreatment solution, and then passing the immersed copper alloy substrate through the molten liquid at a specified rate in an inert environment, and cooling to obtain a copper alloy material.
[0012] As a preferred embodiment of the present invention, the copper alloy raw material includes: 3-4 parts by weight of titanium, 92-96 parts by weight of copper and 0.05-0.1 parts by weight of aluminum or iron.
[0013] As a preferred embodiment of the present invention, the smelting temperature is 1100-1200°C.
[0014] As a preferred embodiment of the present invention, the organic solvent is at least one of fatty acids, aliphatic amines, fatty acid amides, aliphatic alcohols, and esters composed of fatty acids and aliphatic alcohols.
[0015] As a preferred embodiment of the present invention, the prescribed speed is 2-8 m / s.
[0016] As a preferred embodiment of the present invention, the aspect ratio of the nano-carbon fiber is 20-30:1.
[0017] As a preferred embodiment of the present invention, the nano-carbon fiber is further modified, specifically: silicon dioxide, triethylamine, toluene and bromoisobutyryl bromide are dissolved in toluene, reacted at 0-5°C for 3-6h, then continued to react at 20-30°C for 10-13h, centrifuged and dried to obtain product one, product one is reacted with sodium azide and N,N-dimethylformamide at 50-60°C for 20-40h, centrifuged and dried to obtain product two, product two, nano-carbon fiber and N,N-dimethylformamide are added with cuprous bromide in an inert gas atmosphere for reaction, the reaction product is filtered, washed and dried to obtain the product.
[0018] The present invention also discloses a copper alloy material continuous production system for producing the copper alloy material obtained by the above method, comprising a raw material pretreatment system, a smelting furnace, a continuous casting and coating device, and a control system which are arranged in sequence.
[0019] The beneficial effects of the present invention are:
[0020] The present invention discloses a method for producing a copper alloy material, wherein a composite crystalline layer is coated on the surface of a copper alloy substrate, wherein the amorphous layer in the composite crystalline layer contains a plurality of different types of atoms, wherein the disordered structure of the amorphous layer makes it difficult for ions to move, thereby improving the corrosion resistance of the copper alloy. Combined with the nano-carbon fibers mixed in the composite crystalline layer, the bending strength of the copper alloy material is further improved, thereby improving the mechanical strength of the copper alloy. Finally, the carbon fibers are modified to make them more evenly dispersed and more stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic block diagram of the structure of the continuous production system of copper alloy materials of the present invention. DETAILED DESCRIPTION
[0022] A continuous production method of copper alloy material, comprising raw material pretreatment, smelting and continuous casting and cladding;
[0023] Wherein, the continuous casting coating is to coat the surface of the copper alloy substrate obtained after smelting with a composite crystalline layer;
[0024] The preparation method of the composite crystalline layer is as follows:
[0025] S1: dispersing carbon nanofibers in an organic solvent to obtain a pretreatment solution;
[0026] S2: melting the amorphous raw material to obtain a melt;
[0027] S3: Immersing the copper alloy substrate in the pretreatment solution, and then passing the immersed copper alloy substrate through the molten liquid at a specified rate in an inert environment, and cooling to obtain a copper alloy material.
[0028] In some embodiments, the copper alloy raw material includes: 3-4 parts by weight of titanium, 92-96 parts by weight of copper, and 0.05-0.1 parts by weight of aluminum or iron.
[0029] In some embodiments, the smelting temperature is 1100-1200°C.
[0030] In some embodiments, the organic solvent is at least one of a fatty acid, an aliphatic amine, a fatty acid amide, an aliphatic alcohol, and an ester composed of a fatty acid and an aliphatic alcohol.
[0031] In some embodiments, the prescribed rate is 2-8 m / s, specifically, it can be 2, 3, 4, 5, 6, 7 or 8 m / s. If the rate is too fast, the thickness will be too small, which will affect its performance. If the rate is too slow, the thickness will be too large, and there will be a partial transition from amorphous to crystalline state, making it difficult to obtain a completely amorphous coating layer, thereby affecting the corrosion resistance of the copper alloy material.
[0032] In some embodiments, the aspect ratio of the nano-carbon fibers is 20-30:1.
[0033] In some other embodiments, the nano-carbon fiber is further modified, specifically: silica, triethylamine, toluene and bromoisobutyryl bromide are dissolved in toluene, reacted at 0-5°C for 3-6 hours, then continued to react at 20-30°C for 10-13 hours, centrifuged and dried to obtain product one, product one is reacted with sodium azide and N,N-dimethylformamide at 50-60°C for 20-40 hours, centrifuged and dried to obtain product two, product two, nano-carbon fiber and N,N-dimethylformamide are added with cuprous bromide in an inert gas atmosphere to react, the reaction product is filtered, washed and dried to obtain the product.
[0034] The present invention coats a composite crystalline layer on the surface of the copper alloy substrate, wherein the amorphous layer in the composite crystalline layer contains a variety of different types of atoms, wherein the disordered structure of the amorphous layer makes it difficult for ions to move, thereby improving the corrosion resistance of the copper alloy. Combined with the nano-carbon fibers mixed in the composite crystalline layer, the bending strength of the copper alloy material is further improved, thereby improving the mechanical strength of the copper alloy.
[0035] The present invention provides a continuous production system of copper alloy materials, referring to Figure 1 , used to produce the copper alloy material obtained by any of the above methods, including a raw material pretreatment system, a smelting furnace, and a continuous casting and cladding device arranged in sequence, and also including a control system. The control system can give corresponding control signals according to the feedback signals of the raw material pretreatment system, the smelting furnace and the continuous casting and cladding device to realize automatic continuous production.
[0036] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0037] Example 1
[0038] A continuous production method of copper alloy material, comprising raw material pretreatment, smelting and continuous casting and cladding;
[0039] Wherein, the continuous casting coating is to coat the surface of the copper alloy substrate obtained after smelting with a composite crystalline layer;
[0040] The preparation method of the composite crystalline layer is as follows:
[0041] S1: dispersing carbon nanofibers in an organic solvent to obtain a pretreatment solution;
[0042] S2: melting the amorphous raw material to obtain a melt;
[0043] S3: Immersing the copper alloy substrate in the pretreatment solution, and then passing the immersed copper alloy substrate through the molten liquid at a specified rate in an inert environment, and cooling to obtain a copper alloy material.
[0044] The copper alloy raw material includes: 3 parts by weight of titanium, 96 parts by weight of copper and 0.1 parts by weight of aluminum.
[0045] The smelting temperature is 1200°C.
[0046] The organic solvent is coconut oil.
[0047] The prescribed speed is 3 m / s.
[0048] The aspect ratio of the nano-carbon fiber is 30:1.
[0049] The nano-carbon fibers are also modified, specifically: 5 parts by mass of silica, 5 parts by mass of triethylamine, 100 parts by volume of toluene and 5 parts by volume of bromoisobutyryl bromide are dissolved in toluene, reacted at 1°C for 4 hours, then continued to react at 25°C for 12 hours, centrifuged and dried to obtain product one, 4 parts by mass of product one are reacted with 4 parts by mass of sodium azide and 50 parts by volume of N,N-dimethylformamide at 55°C for 25 hours, centrifuged and dried to obtain product two, 3 parts by mass of product two, 10 parts by mass of nano-carbon fibers and 50 parts by volume of N,N-dimethylformamide are added with 2 parts by volume of cuprous bromide to react under an inert gas atmosphere, the reaction product is filtered, washed and dried to obtain the product.
[0050] Example 2
[0051] A continuous production method of copper alloy material, comprising raw material pretreatment, smelting and continuous casting and cladding;
[0052] Wherein, the continuous casting coating is to coat the surface of the copper alloy substrate obtained after smelting with a composite crystalline layer;
[0053] The preparation method of the composite crystalline layer is as follows:
[0054] S1: dispersing carbon nanofibers in an organic solvent to obtain a pretreatment solution;
[0055] S2: melting the amorphous raw material to obtain a melt;
[0056] S3: Immersing the copper alloy substrate in the pretreatment solution, and then passing the immersed copper alloy substrate through the molten liquid at a specified rate in an inert environment, and cooling to obtain a copper alloy material.
[0057] The copper alloy raw material includes: 3 parts by weight of titanium, 96 parts by weight of copper and 0.1 parts by weight of aluminum.
[0058] The smelting temperature is 1200°C.
[0059] The organic solvent is coconut oil.
[0060] The prescribed speed is 4 m / s.
[0061] The aspect ratio of the nano-carbon fiber is 30:1.
[0062] The nano-carbon fibers are also modified, specifically: 5 parts by mass of silicon dioxide, 5 parts by mass of triethylamine, 100 parts by volume of toluene and 5 parts by volume of bromoisobutyryl bromide are dissolved in toluene, reacted at 0-5°C for 4 hours, then continued to react at 25°C for 12 hours, centrifuged and dried to obtain product one, 4 parts by mass of product one are reacted with 4 parts by mass of sodium azide and 50 parts by volume of N,N-dimethylformamide at 50-60°C for 25 hours, centrifuged and dried to obtain product two, 3 parts by mass of product two, 10 parts by mass of nano-carbon fibers and 50 parts by volume of N,N-dimethylformamide are added with 2 parts by volume of cuprous bromide to react under an inert gas atmosphere, the reaction product is filtered, washed and dried to obtain the product.
[0063] Example 3
[0064] A continuous production method of copper alloy material, comprising raw material pretreatment, smelting and continuous casting and cladding;
[0065] Wherein, the continuous casting coating is to coat the surface of the copper alloy substrate obtained after smelting with a composite crystalline layer;
[0066] The preparation method of the composite crystalline layer is as follows:
[0067] S1: dispersing carbon nanofibers in an organic solvent to obtain a pretreatment solution;
[0068] S2: melting the amorphous raw material to obtain a melt;
[0069] S3: Immersing the copper alloy substrate in the pretreatment solution, and then passing the immersed copper alloy substrate through the molten liquid at a specified rate in an inert environment, and cooling to obtain a copper alloy material.
[0070] The copper alloy raw material includes: 3 parts by weight of titanium, 96 parts by weight of copper and 0.1 parts by weight of aluminum.
[0071] The smelting temperature is 1200°C.
[0072] The organic solvent is coconut oil.
[0073] The prescribed speed is 5 m / s.
[0074] The aspect ratio of the nano-carbon fiber is 30:1.
[0075] The nano-carbon fibers are also modified, specifically: 5 parts by mass of silica, 5 parts by mass of triethylamine, 100 parts by volume of toluene and 5 parts by volume of bromoisobutyryl bromide are dissolved in toluene, reacted at 4°C for 5 hours, then continued to react at 25°C for 12 hours, centrifuged and dried to obtain product one, 4 parts by mass of product one are reacted with 4 parts by mass of sodium azide and 50 parts by volume of N,N-dimethylformamide at 55°C for 30 hours, centrifuged and dried to obtain product two, 3 parts by mass of product two, 10 parts by mass of nano-carbon fibers and 50 parts by volume of N,N-dimethylformamide are added with 2 parts by volume of cuprous bromide to react under an inert gas atmosphere, the reaction product is filtered, washed and dried to obtain the product.
[0076] Comparative Example 1
[0077] A continuous production method of copper alloy material, comprising raw material pretreatment, smelting and continuous casting and cladding;
[0078] Wherein, the continuous casting coating is to coat the surface of the copper alloy substrate obtained after smelting with a composite crystalline layer;
[0079] The preparation method of the composite crystalline layer is as follows:
[0080] S1: dispersing carbon nanofibers in an organic solvent to obtain a pretreatment solution;
[0081] S2: melting the amorphous raw material to obtain a melt;
[0082] S3: Immersing the copper alloy substrate in the pretreatment solution, and then passing the immersed copper alloy substrate through the molten liquid at a specified rate in an inert environment, and cooling to obtain a copper alloy material.
[0083] The copper alloy raw material includes: 3 parts by weight of titanium, 96 parts by weight of copper and 0.1 parts by weight of aluminum.
[0084] The smelting temperature is 1200°C.
[0085] The organic solvent is coconut oil.
[0086] The prescribed speed is 5 m / s.
[0087] The aspect ratio of the nano-carbon fiber is 30:1.
[0088] Comparative Example 2
[0089] The change made on the basis of Example 3 is that the specified speed is 15m / s.
[0090] The samples of the above embodiments and comparative examples were subjected to corrosion resistance test and yield strength test, and the test methods are as follows:
[0091] Corrosion resistance test: Based on GB / T 10125-1997, a neutral salt spray test was carried out in a 5% sodium chloride solution environment;
[0092] Yield strength test: The specimen with an aspect ratio of 2:1 was subjected to uniaxial compression test at a compression rate of 5×10 -4 s -1 , the yield strength of the sample was measured, see Table 1 for details.
[0093] Table 1 Performance test results of samples of embodiments and comparative examples
[0094] Sample Yield Strength(Mpa) Corrosion resistance (observe whether there is rust on the surface) Example 1 844 No rust after 150h Example 2 856 No rust after 150h Example 3 847 No rust after 150h Comparative Example 1 712 After 100 hours, rust began to appear Comparative Example 2 754 Corrosion started to occur after 120 hours
[0095] As can be seen from the above table, the performance of the embodiment is better than that of the comparative example. The main reason may be that the embodiment covers a layer of composite crystalline layer on the surface of the copper alloy matrix. The amorphous layer in the composite crystalline layer contains a variety of different types of atoms, and the disordered structure of the amorphous layer makes it difficult for ions to move, thereby improving the corrosion resistance of the copper alloy. Combined with the nano-carbon fibers mixed in the composite crystalline, the bending strength of the copper alloy material is further improved, thereby improving the mechanical strength of the copper alloy. In addition, the carbon fiber is modified to make it more evenly dispersed and more stable. The analysis of comparative example 2 shows that the penetration rate of comparative example 2 may be too fast and the thickness is thin, which affects its performance.
[0096] The above-mentioned embodiments only express the preferred implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all these changes and deformations should fall within the scope of protection of the claims of the present invention.
Claims
1. A method for continuous production of copper alloy materials, characterized in that: Including raw material pretreatment, smelting and continuous casting cladding; Wherein, the continuous casting coating is to coat the surface of the copper alloy substrate obtained after smelting with a composite crystalline layer; The preparation method of the composite crystalline layer is as follows: S1: dispersing carbon nanofibers in an organic solvent to obtain a pretreatment solution; S2: melting the amorphous raw material to obtain a melt; S3: Immersing the copper alloy substrate in the pretreatment solution, and then passing the immersed copper alloy substrate through the molten liquid at a specified rate in an inert environment, and cooling to obtain a copper alloy material.
2. The method for continuous production of copper alloy material according to claim 1, characterized in that: The copper alloy raw material includes: 3-4 parts by weight of titanium, 92-96 parts by weight of copper and 0.05-0.1 parts by weight of aluminum or iron.
3. The method for continuous production of copper alloy material according to claim 1, characterized in that: The smelting temperature is 1100-1200°C.
4. The method for continuous production of copper alloy material according to claim 1, characterized in that: The organic solvent is at least one of fatty acids, aliphatic amines, fatty acid amides, aliphatic alcohols, and esters composed of fatty acids and aliphatic alcohols.
5. The method for continuous production of copper alloy material according to claim 1, characterized in that: The prescribed speed is 2-8 m / s.
6. The method for continuous production of copper alloy material according to claim 1, characterized in that: The aspect ratio of the nano-carbon fiber is 20-30:
1.
7. The method for continuous production of copper alloy material according to claim 1, characterized in that: The nano-carbon fibers are also modified, specifically: silicon dioxide, triethylamine, toluene and bromoisobutyryl bromide are dissolved in toluene, reacted at 0-5°C for 3-6 hours, then continued to react at 20-30°C for 10-13 hours, centrifuged and dried to obtain product one, product one is reacted with sodium azide and N,N-dimethylformamide at 50-60°C for 20-40 hours, centrifuged and dried to obtain product two, product two, nano-carbon fibers and N,N-dimethylformamide are added with cuprous bromide in an inert gas atmosphere for reaction, the reaction product is filtered, and the washing and drying is carried out.
8. A continuous production system for copper alloy materials, used for producing the copper alloy materials obtained by the method according to any one of claims 1 to 7, characterized in that: It includes a raw material pretreatment system, a smelting furnace, a continuous casting and cladding device which are arranged in sequence, and also includes an integrated control system.