Biomass-freeze-dried synergistic carbon nanofiber electrode material as well as preparation method and application thereof

By introducing biomass and lyophilization technologies into carbon nanofiber electrode materials, the problem of difficult to take into account the activity and mass transfer performance of the electrode under high current density is solved, efficient electrochemical reactions and battery performance improvements are achieved, and liquid flow is promoted Stable operation and efficient energy storage of the battery.

CN119020887APending Publication Date: 2024-11-26LIAONING UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411061749.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing carbon nanofiber electrode materials are difficult to take into account both electrochemical activity, conductivity and mass transfer properties under high current density, resulting in the polarization overpotential and concentration polarization of the flow battery under high current density, affecting the stability of the battery. and efficiency.

Method used

Using the preparation method of biomass-freeze-drying synergistic efficiency, fibers are prepared by adding lignin and polyacrylonitrile to the precursor solution, and using ice crystals as support templates during freeze-drying to form high pores The carbon nanofiber electrode material is used to improve the mass-to-load transfer performance of the electrode.

Benefits of technology

It significantly improves the electrochemical reactivity and conductivity of the electrode, enhances the wetting and mechanical strength of the electrode, improves the performance of the flow battery, including improving the battery efficiency and power density, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020887A_ABST
    Figure CN119020887A_ABST
Patent Text Reader

Abstract

The invention discloses a biomass-freeze-dried synergistic carbon nanofiber electrode material as well as a preparation method and application thereof. The preparation method comprises the following steps: adding a proper amount of lignin activated functional components into a mixed solution of polyacrylonitrile (PAN) and N, N-dimethylformamide (DMF) to obtain an electrospinning precursor solution containing lignin, spinning the precursor solution by using an electrospinning technology, collecting into a water coagulating bath, and freeze-drying to prepare loose and porous lignin / PAN three-dimensional nanofibers. And pre-oxidizing and carbonizing the obtained nanofibers in an air atmosphere and a nitrogen atmosphere respectively to obtain the three-dimensional network structure carbon nanofiber electrode material with high active area and high mass transfer performance. When the material is applied to an electrode material of an all-vanadium redox flow battery, battery polarization can be effectively reduced, the power density of the battery and the electrolyte utilization rate are improved, and the preparation method is simple, high in controllability and excellent in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials and energy storage, and specifically relates to a biomass-freeze-dried synergistic carbon nanofiber electrode material and a preparation method and application thereof. Background Art

[0002] Vigorously developing renewable energy is an effective way to solve the problem of excessive consumption of traditional fossil energy. However, the intermittent and volatile nature of renewable energy makes it difficult to directly connect to the grid for use. Safe and efficient large-scale long-term energy storage technology is needed to achieve stable output and efficient use of renewable energy.

[0003] Liquid flow batteries have the unique advantages of intrinsic safety and long-term energy storage, making them one of the preferred technologies for large-scale energy storage. As the site of electrochemical reactions in vanadium batteries, the electrochemical activity and stability of the electrode play a decisive role in the performance and cycle life of liquid flow batteries. Improving the performance of electrode materials to enable batteries to operate efficiently at high current densities is an important way to develop high-power density liquid flow batteries, which also places higher demands on the performance of electrode materials. Therefore, designing and preparing high-performance electrode materials and reducing the polarization overpotential of batteries at high current densities are the key to ensuring the stable operation of batteries at high current densities and are necessary conditions for the development of the next generation of high-power density liquid flow battery stacks.

[0004] Electrospinning technology is an effective means of preparing carbon nanofiber electrode materials, and has been widely used in the design and preparation of flow battery electrode materials in recent years. Compared with the preparation process of commercial carbon felt electrodes, the electrospun carbon nanofiber (ECNFs) electrode has more flexible controllability. The surface composition and structure of the carbon nanofiber electrode can be achieved by regulating the composition of the electrospinning precursor solution, thereby improving the surface activity and stability of the electrode.

[0005] However, it is difficult to adjust the surface composition and structure of the fiber alone to take into account the sharp increase in concentration polarization of the electrode at high current density. In addition, the diameter of the carbon fiber prepared by electrospinning technology is hundreds of nanometers, and the structure is more compact, which makes the electrode have low porosity and poor permeability, seriously hindering the transmission of electrolyte inside the electrode. Therefore, it is necessary to improve the three-dimensional pore structure of the electrode while improving the surface activity of the electrode, so as to take into account the activation polarization and concentration polarization of the battery at the same time, so that it can operate stably and efficiently at higher current density.

[0006] In order to solve the above problems, the present invention uses a simple and controllable electrospinning technology, by introducing lignin functional components with rich oxygen-containing functional groups and conjugated aromatic structures into the precursor solution, enhancing the fiber strength while giving the material good surface hydrophilicity and catalytic activity, thereby effectively improving the electrochemical reaction activity of the electrode material; on the other hand, by adopting the coagulation bath-freeze drying technology, the fiber is collected in a water coagulation bath, and ice crystals are used as fiber support templates during the freeze drying process to achieve the construction of high-porosity electrospun carbon nanofibers, thereby obtaining a porous carbon nanofiber electrode material with high mass transfer and charge transfer performance. Using it as a flow battery electrode material can effectively improve the mass transfer rate of the electrolyte in the electrode and the electrochemical reaction rate on the electrode surface, thereby improving the battery efficiency and power density. Summary of the invention

[0007] In view of the problem that it is difficult to balance the activity, conductivity and mass transfer performance of current carbon nanofiber electrode materials, the present invention proposes to use biomass as an activation functional component and coagulation bath-freeze drying as a mass transfer enhancement technology to effectively improve the mass transfer-charge transfer performance of the electrode, taking into account the activation polarization, ohmic polarization and concentration polarization of the battery during the charge and discharge process, thereby improving the performance of the liquid flow battery.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A biomass-freeze-dried synergistic carbon nanofiber electrode material, the preparation method of which comprises the following steps:

[0010] 1) mixing lignin, polyacrylonitrile (PAN) and N,N-dimethylformamide (DMF) to obtain an electrospinning precursor solution containing lignin;

[0011] 2) electrospinning with an electrospinning precursor solution containing lignin, and collecting the fiber precursors into a conductive container containing a water coagulation bath;

[0012] 3) pre-freezing the collected fiber precursors together with the water coagulation bath, and then placing them in a freeze dryer for freeze drying to obtain original nanofibers;

[0013] 4) pre-oxidizing the original nanofibers to obtain pre-oxidized nanofibers;

[0014] 5) The pre-oxidized nanofibers are carbonized to obtain a biomass-freeze-dried synergistic carbon nanofiber electrode material.

[0015] Furthermore, in the above-mentioned method for preparing a biomass-freeze-dried synergistic carbon nanofiber electrode material, in step 1), the molecular weight of the polyacrylonitrile PAN is 60,000 to 150,000.

[0016] Furthermore, in the above-mentioned method for preparing a biomass-freeze-dried synergistic carbon nanofiber electrode material, in step 1), the lignin is dealkalized lignin.

[0017] Furthermore, in the above-mentioned method for preparing a biomass-freeze-dried synergistic carbon nanofiber electrode material, in step 1), in the mixed solution of lignin, polyacrylonitrile PAN and N,N-dimethylformamide DMF, the concentration of polyacrylonitrile PAN is 10-18wt%, and the concentration of lignin is 0.6-1wt%.

[0018] Furthermore, in the above-mentioned method for preparing a biomass-freeze-dried synergistic carbon nanofiber electrode material, in step 1), the mixing conditions are controlled as follows: temperature is 70-90° C., and magnetic stirring is performed for 12-24 hours.

[0019] Furthermore, in the above-mentioned method for preparing a biomass-freeze-dried synergistic carbon nanofiber electrode material, in step 2), the process conditions of the electrospinning are: voltage of 10-20 kV; receiving distance of 3-10 cm; nozzle moving distance of 50-500 mm; nozzle moving speed: 5-20 mm / s; spinning temperature of 15-30°C; spinning humidity of 10-50% RH; push speed of 10-50 μL / min; spinning time of 0.5-10 h.

[0020] Furthermore, in the above-mentioned method for preparing a biomass-freeze-dried synergistic carbon nanofiber electrode material, in step 3), the freeze-drying conditions are: first freezing at -20 to -60°C for 5 to 24 hours, and then freeze-drying at -40 to -80°C for 5 to 24 hours.

[0021] Furthermore, in the above-mentioned method for preparing a biomass-freeze-dried synergistic carbon nanofiber electrode material, in step 4), the process conditions of the pre-oxidation treatment are: heat treatment at 250-350° C. for 0.5-3 h in an air atmosphere.

[0022] Furthermore, in the above-mentioned method for preparing a biomass-freeze-dried synergistic carbon nanofiber electrode material, in step 5), the process conditions of the carbonization treatment are: heat treatment at 900-1200° C. for 1-5 hours in a vacuum, nitrogen or argon atmosphere.

[0023] Application of any of the above-mentioned biomass-freeze-dried synergistic carbon nanofiber electrode materials in liquid flow batteries.

[0024] Furthermore, in the above application, the flow battery includes an all-vanadium flow battery, a zinc-bromine flow battery, an all-iron flow battery, an iron-chromium flow battery and an organic flow battery.

[0025] The beneficial effects of the present invention are:

[0026] 1. The preparation method of the biomass-freeze-dried synergistic carbon nanofiber electrode proposed in the present invention is simple, flexible in operation, economical and environmentally friendly, and has universal applicability.

[0027] 2. The biomass-freeze-dried synergistic carbon nanofiber electrode proposed in the present invention has more surface active sites for the carbon nanofibers during the pyrolysis of the biomass. The coagulation bath freeze-drying process enables a thin carbon layer to be generated on the surface of the fiber during the subsequent heat treatment. The thin carbon layer has a more ordered graphite microcrystalline structure, and the electrical conductivity is effectively improved. The freeze-dried fiber has a more fluffy porous structure, which can significantly improve the wettability of the electrode material, promote the contact between the electrolyte and the electrode, and thereby improve the mass transfer performance of the electrode.

[0028] 3. The present invention proposes to utilize a large number of hydroxyl and carboxyl groups in the lignin structure to form a multi-level hydrogen bond network with polyacrylonitrile-based fibers, thereby reducing fiber breakage during heat treatment and helping to improve the mechanical strength of carbon fiber materials.

[0029] 4. In addition, as an economical and environmentally friendly biomass material, the application of lignin in electrochemical energy storage electrode materials can further broaden its application field and realize high value-added utilization of biological waste.

[0030] 5. The preparation technology of the biomass-freeze-dried synergistic carbon nanofiber electrode material proposed in the present invention has broad application prospects in liquid flow batteries, and is of great significance for improving the performance of liquid flow batteries and promoting the industrialization development of clean energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Scanning electron microscope images of blank polyacrylonitrile carbon nanofiber electrode material (ECNFs) (a) and biomass-freeze-dried synergistic carbon nanofiber electrode material (WL-ECNFs) (b) prepared in Example 1.

[0032] Figure 2 Cyclic voltammetry curves of blank polyacrylonitrile carbon nanofiber electrode material (ECNFs) and biomass-freeze-dried synergistic carbon nanofiber electrode material (WL-ECNFs) prepared in Example 1 in 0.1M VOSO4+2M H2SO4 (scan rate: 5mV·s -1 )(a) and electrochemical impedance Nyquist curve and corresponding equivalent circuit diagram (polarization voltage: -0.5V(b) and 0.9V(c)).

[0033] Figure 3Polarization curves of single cells assembled from blank polyacrylonitrile carbon nanofiber electrode materials (ECNFs) and biomass-freeze-dried synergistic carbon nanofiber electrode materials (WL-ECNFs) prepared in Example 1 (a) and at 250 mA·cm -2 The charge and discharge curves under different current densities (b) and the Coulombic efficiency CE, voltage efficiency VE and energy efficiency EE at different current densities (c). DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0035] Example 1

[0036] (I) Comparative Example - Preparation of Blank Polyacrylonitrile Carbon Nanofiber Electrode Material

[0037] 1) After drying polyacrylonitrile (PAN) powder with a molecular weight of 150,000, it is mixed with N,N-dimethylformamide (DMF) solution and magnetically stirred at 80°C for 10 hours until it is completely dissolved to obtain a mixed solution of polyacrylonitrile (PAN) and N,N-dimethylformamide (DMF) with a mass percentage concentration of polyacrylonitrile (PAN) of 12wt% (PAN / DMF solution), which is used as an electrospinning precursor solution.

[0038] 2) Put the electrospinning precursor solution PAN / DMF into a syringe and place it on the syringe pump, and connect the pipeline. Electrospinning conditions: voltage 20KV; roller as fiber receiver; distance between stainless steel flat needle and receiver 10cm; nozzle moving speed 10mm / s; nozzle moving distance 30mm; spinning temperature 30℃; spinning humidity 40%RH; push speed 25μL / min; spinning time 2h. After setting the electrospinning parameters, electrospinning was started to obtain blank polyacrylonitrile electrospun nanofibers.

[0039] 3) Pre-oxidation treatment: The blank polyacrylonitrile electrospun nanofibers were heat treated at 290°C for 1 h in an air atmosphere. The pre-oxidation treated samples were then heat treated at 1000°C for 2 h in a nitrogen atmosphere. After cooling, blank polyacrylonitrile carbon nanofiber electrode materials were obtained. Figure 1 As shown in (a), the blank polyacrylonitrile carbon nanofiber electrode material (ECNFs) has a smooth fiber surface and a diameter of about 276 nm.

[0040] (II) Preparation of biomass-freeze-dried synergistic carbon nanofiber electrode materials (WL-ECNFs)

[0041] 1) According to the mass ratio of dealkalized lignin: polyacrylonitrile = 1:14, dried polyacrylonitrile (PAN) powder with a molecular weight of 150,000 and dealkalized lignin powder are dissolved in N,N-dimethylformamide (DMF) solvent, and mixed with magnetic stirring at 80°C for 12 hours to prepare an electrospinning precursor solution with a mass percentage of polyacrylonitrile of 14wt% and a mass percentage of dealkalized lignin of 1wt%, and the mixed solution is used as an electrospinning precursor solution.

[0042] 2) Put the electrospinning precursor solution into a syringe and place it on a syringe pump, connect the pipeline, and use deionized water as a coagulation bath solution to collect the fiber precursors. Electrospinning conditions: voltage 14kV; iron box with aluminum foil as a fiber receiver; the distance between the stainless steel flat needle and the receiver is 5cm; nozzle movement speed 10mm / s; nozzle movement distance 100mm; spinning temperature 30℃; spinning humidity 30% RH; push speed 25μL / min; spinning time 30min. After setting the electrospinning parameters, start electrospinning and collect the fiber precursors into an iron box with aluminum foil filled with deionized water.

[0043] 3) The collected fiber precursors are placed in a refrigerator together with deionized water and then placed in a freeze dryer. They are first frozen in a refrigerator at -20°C for 6 hours to maintain the loose porous structure of the fiber; then placed in a freeze dryer at -55°C for vacuum drying for 12 hours to obtain fluffy original nanofibers. The fluffy original nanofibers are placed between corundum plates and placed in a box furnace for pre-oxidation treatment, that is, heat treated at 290°C for 60 minutes in an air atmosphere to obtain pre-oxidized nanofibers.

[0044] 4) The obtained pre-oxidized nanofibers were carbonized by heat treating them at 1000° C. for 120 min in a nitrogen atmosphere to obtain a biomass-freeze-dried synergistic carbon nanofiber electrode material, which was labeled as WL-ECNFs.

[0045] like Figure 1 (b) shows: WL-ECNFs have more cross-linked structures, the fibers are bundle-shaped, and their diameter is smaller than that of ECNFs, about 220nm.

[0046] Example 2 Electrochemical performance of biomass-freeze-dried synergistic carbon nanofiber electrode materials (WL-ECNFs)

[0047] 1) Cyclic voltammetry (CV) test and electrochemical impedance spectroscopy (EIS) test

[0048] Method: The electrochemical performance of the material was tested using a three-electrode system. 2The material-freeze-dried synergistically enhanced carbon nanofiber electrode material (WL-ECNFs) and blank polyacrylonitrile carbon nanofiber electrode material (ECNFs) were used as working electrodes; 232 type saturated calomel electrode was used as reference electrode; platinum sheet was used as auxiliary electrode, and 0.1M VOSO4+2.0M H2SO4 was used as electrolyte.

[0049] Figure 2 (a) is the measured cyclic voltammetry (CV) curve. The reaction current of the electrode material WL-ECNFs obtained by the coagulation bath combined with freeze-drying technology to the positive and negative vanadium ion redox couple is significantly larger than that of ECNFs, and the redox peak position difference is reduced, indicating that it not only has excellent electrochemical activity but also has increased electrochemical reversibility. At the same time, it is found that its double layer capacitance is also greater than that of ECNFs, which once again shows that the three-dimensional network structure obtained by the coagulation bath combined with freeze-drying technology can effectively increase the effective reaction area of ​​the material, which is beneficial to the penetration of active components and thus improves the electrode reaction kinetics.

[0050] The electrochemical properties of the material were further studied by electrochemical impedance spectroscopy. The polarization potentials of the positive and negative electrodes were 0.9V and -0.5V, respectively. Figure 2 (bc) shows the Nyquist curves and corresponding equivalent circuits of the negative and positive electrodes of ECNFs and WL-ECNFs. The Nyquist plots of both materials contain two semicircular arcs and a linear part, indicating that the electrochemical reaction of vanadium ions on the surface of each electrode is controlled by a mixture of charge transfer and diffusion processes, and WL-ECNFs has a smaller semicircular arc, indicating that it has lower interface resistance and charge transfer resistance, which is consistent with the CV test results.

[0051] 2) Battery charge and discharge test

[0052] Method: The biomass electrospun carbon nanofiber electrode material (WL-ECNFs) with high mass transfer and charge transfer performance prepared in Example 1 was used as the positive and negative electrode materials, and the area of ​​the working electrode was 2×2 cm 2 , Nafion 212 is an ion exchange membrane, 1.65MV 3.5+ +3.0M H2SO4 as electrolyte, assemble a single cell. The blank polyacrylonitrile carbon nanofiber electrode material prepared in Example 1 was used as the control group, the blank polyacrylonitrile carbon nanofiber electrode material ECNFs was used as the positive and negative electrodes, and the area of ​​the working electrode was 2×2 cm 2 , Nafion 212 is an ion exchange membrane, 1.65MV 3.5+ +3.0M H2SO4 as electrolyte, assembled single cell. The charge and discharge cut-off voltages are 1.75V and 1.0V respectively. The polarization curve, charge and discharge curve and battery efficiency of the battery are shown in Figure 3 shown.

[0053] like Figure 3 As shown in (a), the WL-ECNFs assembled battery exhibits a higher power density than the battery assembled with blank ECNFs electrode materials, with a peak power density of 697 mW cm -2 , the latter is 620mW·cm -2 .like Figure 3 (b) shows that the WL-ECNFs battery is at 250 mA cm -2 The batteries assembled with ECNFs exhibit lower polarization overpotential and higher charge-discharge capacity than those assembled with blank ECNFs. Figure 3 (c) Coulombic efficiency CE, voltage efficiency VE and energy efficiency EE of WL-ECNFs at different current densities. The results show that the battery can still operate smoothly at higher current densities and has a good performance at 200 mA cm -2 The voltage efficiency and energy efficiency of the battery reached 82.7% and 79.2%, respectively, which are significantly better than those of the battery assembled with ECNFs.

Claims

1. A biomass-freeze-dried synergistic carbon nanofiber electrode material, characterized in that: The preparation method thereof comprises the following steps: 1) mixing lignin, polyacrylonitrile (PAN) and N,N-dimethylformamide (DMF) to obtain an electrospinning precursor solution containing lignin; 2) electrospinning with an electrospinning precursor solution containing lignin, and collecting the fiber precursors into a conductive container containing a water coagulation bath; 3) pre-freezing the collected fiber precursors together with the water coagulation bath, and then placing them in a freeze dryer for freeze drying to obtain original nanofibers; 4) pre-oxidizing the original nanofibers to obtain pre-oxidized nanofibers; 5) The pre-oxidized nanofibers are carbonized to obtain a biomass-freeze-dried synergistic carbon nanofiber electrode material.

2. The biomass-freeze-dried synergistic carbon nanofiber electrode material according to claim 1, characterized in that: In step 1), the molecular weight of the polyacrylonitrile (PAN) is 60,000 to 150,000; and the lignin is dealkalized lignin.

3. The biomass-freeze-dried synergistic carbon nanofiber electrode material according to claim 1, characterized in that: In step 1), in the mixed solution of lignin, polyacrylonitrile PAN and N,N-dimethylformamide DMF, the concentration of polyacrylonitrile PAN is 10-18 wt %, and the concentration of lignin is 0.6-1 wt %.

4. The biomass-freeze-dried synergistic carbon nanofiber electrode material according to claim 1, characterized in that: In step 1), the mixing conditions are controlled as follows: temperature is 70-90° C., and magnetic stirring is performed for 12-24 hours.

5. The biomass-freeze-dried synergistic carbon nanofiber electrode material according to claim 1, characterized in that: In step 2), the process conditions of the electrospinning are: voltage of 10-20 kV; receiving distance of 3-10 cm; nozzle moving distance of 50-500 mm; nozzle moving speed: 5-20 mm / s; spinning temperature of 15-30°C; spinning humidity of 10-50% RH; push speed of 10-50 μL / min; spinning time of 0.5-10 h.

6. The biomass-freeze-dried synergistic carbon nanofiber electrode material according to claim 1, characterized in that: In step 3), the freeze-drying conditions are: first freezing at -20 to -60°C for 5 to 24 hours, and then freeze-drying at -40 to -80°C for 5 to 24 hours.

7. The biomass-freeze-dried synergistic carbon nanofiber electrode material according to claim 1, characterized in that: In step 4), the process conditions of the pre-oxidation treatment are: heat treatment at 250-350° C. for 0.5-3 h in an air atmosphere.

8. The biomass-freeze-dried synergistic carbon nanofiber electrode material according to claim 1, characterized in that: In step 5), the process conditions of the carbonization treatment are: heat treatment at 900-1200° C. for 1-5 hours in a vacuum, nitrogen or argon atmosphere.

9. Use of the biomass-freeze-dried synergistic carbon nanofiber electrode material according to any one of claims 1 to 8 in a liquid flow battery.

10. The use according to claim 9, characterized in that: The flow batteries include all-vanadium flow batteries, zinc-bromine flow batteries, all-iron flow batteries, iron-chromium flow batteries and organic flow batteries.

Citation Information

Cited By

  • Electrospinning carbon nanofiber electrode material with high mass transfer-charge transfer performance as well as preparation method and application of electrospinning carbon nanofiber electrode material

    CN116623320A

  • Method for preparing carbon nanofibers from polysaccharide biomass

    CN120625223A