Janus-like structure difunctional nanofiber and preparation method thereof

Janus-like nanofibers were prepared on hollow porous carbon fibers using coaxial spinning and in-situ growth techniques. This solved the problems of few active sites and poor stability, enabling the application of highly efficient bifunctional materials in electrocatalysis, electromagnetic shielding, and sensing.

CN119041056APending Publication Date: 2024-11-29HENAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411168641.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing Janus-structured nanofiber materials suffer from a lack of active sites and poor stability. In particular, during the preparation process, the active sites are often coated or the content of functional materials is low, resulting in insufficient functionality of the materials.

Method used

By combining coaxial spinning and in-situ growth techniques, different functional materials are grown on the inner and outer sides of hollow porous carbon fibers. Through the carbonization process of high carbon yield polymers and pyrolytic polymers, the core functional material is exposed, and the outer material is grown in situ, forming bifunctional nanofibers with abundant active sites and high stability, resembling the Janus structure.

Benefits of technology

This study achieves the enrichment and improved stability of active sites in nanofiber materials, resulting in highly efficient bifunctional fibers suitable for fields such as electrocatalysis, electromagnetic shielding, and sensing. Furthermore, the preparation process is simple, economical, and yields large quantities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041056A_ABST
    Figure CN119041056A_ABST
Patent Text Reader

Abstract

The invention provides a Janus-like structure difunctional nanofiber and a preparation method thereof, belongs to the technical field of nanofiber materials, and aims to solve the technical problems of few active sites and poor stability of Janus structure nanofibers. The preparation method of the functional nanofiber comprises the following steps: (1) mixing and dissolving a high-carbon-yield polymer I, a pyrolysis type polymer, a functional material and a solvent I to obtain a first spinning solution; (2) mixing and dissolving a high-carbon-yield polymer II and a solvent II to obtain a second spinning solution; (3) spinning by taking the first spinning solution as an internal solution and the second spinning solution as an external solution in a coaxial spinning manner to obtain a core-shell structure polymer fiber membrane precursor; (4) soaking the core-shell structure polymer fiber membrane precursor in the prepared growth solution to obtain a Janus-like structure difunctional polymer nanofiber; and (5) calcining and carbonizing the difunctional polymer nanofiber with the similar Janus structure, so as to obtain the difunctional carbon nanofiber with the similar Janus structure. The hollow porous carbon fiber is used as a substrate, different functional materials grow on the inner side and the outer side respectively, and the prepared functional nanofiber has the advantages of being rich in active material and high in stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanofiber materials, and in particular relates to a Janus-like structure dual-function nanofiber and a preparation method thereof. Background Art

[0002] With the accelerated evolution of a new round of scientific and technological revolution and industrial transformation, people are increasingly demanding high-performance and dual-functional materials to meet the needs of green and sustainable development. The redox reactions corresponding to the battery charging and discharging process, the carbon dioxide hydrogenation reaction, and the reforming catalysis in the petrochemical industry have the problem of slow reaction kinetics, resulting in low energy conversion efficiency. On the other hand, the single function of the current materials leads to complex device structure and increased device weight. Efficient dual-functional materials are the key to improving energy conversion efficiency and device integration, and are also the current focus of research and application. Janus structure materials refer to a material with clear structural characteristics on the two surfaces and different properties such as hydrophilicity / hydrophobicity, oxidizability / reduction, conductivity / insulation, electronegativity / electropositivity, etc., which can meet the needs of dual functions, but there are still problems of few active sites and poor stability. Therefore, it is of great significance to develop a Janus-like dual-functional nanofiber material with rich active sites and high stability.

[0003] At present, there are three main methods for preparing Janus-like bifunctional materials. The first is to spray, grow in situ or adsorb two materials with different properties on both sides of the matrix material. The physical adsorption method has the problem of easy detachment, resulting in poor material stability. The in-situ grown Janus structure material has excellent stability, but the matrix for adsorption and in-situ growth is usually in the form of a film or block, and the functional material only exists on the surface of the film or block, resulting in a low content of functional materials. The second method is to disperse the functional material in the spinning solution for spinning, first prepare a functional fiber membrane, and then spin another functional fiber on this basis to prepare a bifunctional Janus structure fiber membrane. This method can spin any dispersible functional material, with a wide range of selection and excellent stability, but the functional material is coated by the spinning solution, resulting in a small number of active sites in the material. The third method is to directly prepare bifunctional nanofibers with a Janus-like structure. For example, by utilizing the phase separation phenomenon of the solution, a hydrophilic / hydrophobic solution is electrospun to prepare a bifunctional material. Adding functional particles to the spinning solution can make the fiber functional, but there is also the problem of active sites being coated. Therefore, it is imperative to develop efficient and stable bifunctional nanofibers with a Janus-like structure.

[0004] Patent publication number CN 113990673A discloses a positive and negative electrode integrated Janus structure fiber aerogel and its preparation method, and prepares PAN-PS-ZIF67 / PAN-PS-Fe by coaxial electrospinning. 3+ Based on Janus structure fiber membrane, multi-channel carbon nanofibers with Co3O4 embedded on one side and FeO embedded on the other side were prepared by shear homogenization, freeze drying, carbonization and oxidation heat treatment. x Janus structure fiber aerogel. However, there is also the problem of active sites being coated. Summary of the invention

[0005] In order to solve the technical problems of few active sites and poor stability of Janus structure nanofibers, the present invention proposes a Janus structured bifunctional nanofiber and a preparation method. The hollow porous carbon fiber is used as a substrate, and different functional materials are grown on the inner and outer sides respectively. The prepared functional nanofiber has the characteristics of rich active materials and high stability.

[0006] In order to achieve the above object, the technical solution of the present invention is achieved as follows:

[0007] A Janus-like bifunctional nanofiber, the preparation method of which comprises the following steps:

[0008] Step 1, mixing and dissolving a high carbon yield polymer I, a pyrolysis polymer, a functional material and a solvent I to obtain a first spinning solution;

[0009] Step 2, mixing and dissolving the high carbon yield polymer II and the solvent II to obtain a second spinning solution;

[0010] Step 3, using the first spinning solution as the inner solution and the second spinning solution as the outer solution, spinning is performed by coaxial spinning to obtain a core-shell structure polymer fiber membrane precursor;

[0011] Step 4, placing the core-shell structure polymer fiber membrane precursor into the configured growth solution and soaking it to obtain Janus-like bifunctional polymer nanofibers;

[0012] Step 5, collecting the Janus-like bifunctional polymer nanofibers and transferring them to a vacuum drying oven for drying;

[0013] Step 6, placing the dried Janus-like bifunctional polymer nanofibers into a tubular furnace, first calcining them in air, and then carbonizing them in a certain gas atmosphere to obtain Janus-like bifunctional nanocarbon fibers;

[0014] Preferably, the functional material in step 1 is one or more of functional salts, metal organic frameworks, Prussian blue-like compounds, hydroxides, oxides, sulfides and selenides, and the functional salts are nitrates, chlorides, sulfates, acetates or acetylacetonates; and the pyrolytic polymer is one or more of polymethyl methacrylate and polystyrene.

[0015] The high carbon yield polymer I and high carbon yield polymer II are respectively selected from one or more of polyacrylonitrile, polyvinyl pyrrolidone and polyvinyl alcohol; the solvent I and solvent II are respectively selected from one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide and ionic liquid.

[0016] The mass ratio of the high carbon yield polymer I, the pyrolysis polymer and the functional material is 1:(1-5):(0.1-5), the total concentration of the solute in the first spinning solution is 5-30wt%; the concentration of the high carbon yield polymer II in the second spinning solution is 5-30wt%.

[0017] The temperature during dissolution in the steps 1 and 2 is 60-90° C. and the time is 4-48 hours.

[0018] The coaxial spinning is coaxial electrostatic spinning, coaxial wet spinning or coaxial dry spinning.

[0019] The electrospinning voltage is 8-30kV, the distance between the needle and the receiver is 10-40cm, the roller receiver speed is 50-3000r / min, the core solution injection speed is 0.5-3ml / h, the shell solution injection speed is 0.5-3ml / h, the temperature is 15-40℃, and the humidity is 20-40%; the dry spinning and wet spinning injection speeds are the same as those of electrospinning, and the total traction ratio is 1-20.

[0020] Preferably, the growth solution in step 4 is a one-dimensional, two-dimensional, or three-dimensional material solution system that can be grown in situ, such as a metal organic framework, a Prussian blue, a hydroxide, an oxide, a sulfide, a selenide, or the like, as well as one or more other material solutions that can form chemical bonds and physical adsorption; the immersion method is one or more of standing, stirring, and ultrasound; the immersion time is 2-24 hours; and the immersion temperature is 25-150°C.

[0021] Preferably, the drying temperature in step 5 is 40-80° C., and the drying time is 6-24 hours.

[0022] Preferably, in step six, the calcination is first carried out in an air atmosphere, with a heating rate of 0.5-10°C / min, a calcination temperature of 150-280°C, and a calcination time of 1-3h; the carbonization atmosphere includes one or more of nitrogen, argon, hydrogen, and ammonia; the heating rate is 0.5-10°C / min; the carbonization temperature is 500-1500°C, the carbonization time is 1-4h, and the furnace is naturally cooled to room temperature.

[0023] Beneficial effects of the present invention:

[0024] First, the present invention adopts a method combining coaxial spinning technology and in-situ treatment technology. The pyrolysis polymer is decomposed after carbonization, which causes the functional material of the core layer to be exposed. Therefore, the functional material of the core layer has a large number of active sites. The high carbon yield polymer in the core layer is carbonized to form porous carbon. The porous carbon serves as a supporting structure to load the inner layer functional material. The core layer functional material has high stability. The fiber precursor is a polymer fiber, and the fiber surface contains a large number of functional groups, which provides the possibility for subsequent in-situ growth. The outer layer functional material adopts the in-situ growth method. The in-situ grown material has the characteristics of many active sites and strong bonding with the matrix. The final fiber has the characteristics of rich active materials and high stability, which fundamentally solves the problems of difficult preparation, low yield, and poor stability of Janus structure nanofibers.

[0025] Second, the technical solution of the present invention is economical, simple and universal. (1) The equipment involved in the technical solution is magnetic stirring, vacuum drying oven, spinning machine and tubular furnace, etc., and the equipment is inexpensive; the spinning process can prepare nanofibers in large quantities and continuously, and the fiber material preparation process is stable and has a large output. (2) Functional particles or salts that can be dispersed in the solution can be introduced into the core layer, and any material that can be grown in situ can be introduced into the outer layer. The function of the Janus structural material is universal and designable. (3) The prepared fibers can be further processed, such as vulcanization, nitridation, etc., and the prepared Janus structural fibers are self-supporting membrane materials that avoid the use of binders, expand the application field, and have certain commercial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 The scanning electron microscope image of the core layer nickel-iron metal-modified nanorods and the outer layer leaf-shaped cobalt-based metal organic framework-derived hollow Janus-like structure bifunctional nanofibers obtained in Example 1;

[0028] Figure 2 The transmission electron micrograph of the nanorods modified with nickel-iron metal in the core layer and the hollow Janus-like bifunctional nanofibers derived from the leaf-like cobalt-based metal organic framework in the outer layer obtained in Example 1;

[0029] Figure 3 This is a comparison chart of the oxygen reduction reaction and oxygen evolution reaction performance of the hollow Janus-like bifunctional nanofiber obtained in Example 1 in 0.1M KOH solution and the performance of the corresponding commercial precious metals. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] A Janus-like bifunctional nanofiber, the preparation method of which comprises the following steps:

[0033] Polyacrylonitrile was dissolved in dimethylformamide under continuous magnetic stirring at 60°C for 12 hours to obtain a 10% mass fraction solution A; polyacrylonitrile, polymethyl methacrylate, nickel nitrate and ferric chloride were dissolved in dimethylformamide in a mass ratio of 2:6:1:1 under continuous magnetic stirring at 90°C for 12 hours to obtain a 12% mass fraction solution B.

[0034] Solution A was used as the shell solution and solution B as the core solution, respectively, and added into a 25 ml syringe, with injection speeds of 1 ml / h and 0.5 ml / h, respectively, and the spinning voltage was 8 kV, the distance between the spinneret and the receiver was 10 cm, the receiver speed was 50 rpm, the temperature was 15 ° C, and the humidity was 20% for spinning parameters to obtain a core-shell structure polymer fiber precursor. The fiber was dried in a vacuum oven at 80 ° C for 6 hours.

[0035] 12mmol of dimethylimidazole was added to 40ml of deionized water, and the solution was continuously stirred at room temperature for 30min to obtain solution C; the stirring speed of solution C was adjusted to 100rpm, and the core-shell polymer fiber cut into a certain size was placed in solution C and soaked for 30min; 2.5mmol of cobalt nitrate was added to 40ml of deionized water, and the solution was continuously stirred at room temperature for 30min to obtain solution D; solution D was slowly added to solution C and stirred for 2h, and then allowed to stand for 2h. The fiber was washed three times with ethanol and dried in a vacuum oven at 60℃ for 12h.

[0036] The temperature was first raised to 150°C in an air atmosphere at a heating rate of 1°C / min and maintained for 3 hours, then raised to 800°C in a nitrogen atmosphere at a heating rate of 1°C / min and maintained for 2 hours, and then cooled to room temperature with the furnace to obtain a porous nanorod modified with nickel-iron metal as the core layer, carbon nanofibers as the shell layer, and Janus-like bifunctional nanofibers derived from a leaf-shaped cobalt-based metal-organic framework as the outer layer.

[0037] Figure 1 This is a scanning electron microscope image of a hollow Janus-like bifunctional nanofiber. After carbonization, the fiber still maintains a continuous structure ( Figure 1 a). Figure 1 The partial enlarged image of a shows that the carbonized fiber has a hollow structure, the outer leaf-shaped cobalt-based metal organic framework derivative is tightly attached to the outer surface of the hollow fiber, and the core layer of nickel-iron metal-modified porous nanorods is tightly attached to the inner surface of the hollow fiber ( Figure 1 b). The tight structure of the inner and outer layers of the hollow fiber makes the fiber have a certain stability, which further proves that the method provided by the present invention has a certain feasibility. The transmission electron microscopy image of the hollow Janus-like bifunctional nanofiber further shows that the leaf-shaped cobalt-based metal organic framework derivative is tightly attached to the outer surface of the fiber, and there are a large number of nanoparticles of about 18nm inside the fiber leaf-shaped sheet ( Figure 2 ). The hollow Janus-like bifunctional nanofibers and commercial precious metals were tested in 0.1M KOH solution to evaluate the fiber performance. Figure 3 As shown in a, the half-wave potential of the oxygen reduction reaction of the hollow Janus-like bifunctional nanofibers is 0.87V, which is better than the 0.85V half-wave potential of commercial precious metal Pt / C. Figure 3 As shown in Fig. b, the oxygen evolution reaction overpotential of the hollow Janus-like bifunctional nanofiber is 336 mV, which is better than the 337 mV overpotential of the commercial noble metal RuO2. The inner and outer layers of the fiber prepared by the present invention are tightly attached to the hollow fiber, which is beneficial to the transmission of electrons. The outer leaf-like structure and the core porous structure allow the fiber to have more contact area with the electrolyte, so that the hollow Janus-like bifunctional nanofiber has excellent oxygen reduction reaction and oxygen evolution reaction performance.

[0038] Example 2

[0039] A Janus-like bifunctional nanofiber, the preparation method of which comprises the following steps:

[0040] Polyvinyl pyrrolidone was dissolved in dimethylformamide under continuous magnetic stirring at 90°C for 4 hours to obtain a 30% mass fraction solution A; polyvinyl alcohol, polymethyl methacrylate, copper sulfate, zinc acetate and ferric acetylacetonate were dissolved in dimethylformamide at a mass ratio of 1:3:1:1:1 under continuous magnetic stirring at 80°C for 24 hours to obtain a 30% mass fraction solution B.

[0041] Solution A was used as the shell solution and solution B as the core solution, respectively, and added into a 25 ml syringe, with injection speeds of 3 ml / h and 1.5 ml / h, respectively, and the spinning voltage was 30 kV, the distance between the spinneret and the receiver was 40 cm, the receiver speed was 3000 rpm, the temperature was 40°C, and the humidity was 20% for spinning to obtain a core-shell structure polymer fiber precursor. The fiber was dried in a vacuum oven at 70°C for 12 hours.

[0042] 1.2mmol of cobalt nitrate, 0.6mmol of iron nitrate, 5mmol of ammonium fluoride and 10mmol of urea were added to 40ml of deionized water, and the solution C was obtained by continuous magnetic stirring at room temperature for 30min. The stirring speed of solution C was adjusted to 100rpm, and the core-shell structure polymer fiber cut into a certain size was placed in solution C for ultrasonic immersion for 30min. The fiber and the solution were poured into a reactor and reacted at 150℃ for 8h. After cooling to room temperature, the fiber was washed three times with ethanol and dried in a vacuum oven at 70℃ for 12h.

[0043] The temperature was first raised to 280°C in an air atmosphere at a heating rate of 0.5°C / min and maintained for 1 hour, then raised to 600°C in an ammonia atmosphere at a heating rate of 0.5°C / min and maintained for 1 hour, and then cooled to room temperature with the furnace to obtain a core layer of porous nanorods modified with copper, zinc and iron metals, a shell layer of carbon nanofibers, and an outer layer of Janus-structured bifunctional nanofibers derived from flaky cobalt-iron-based metal hydroxides.

[0044] Example 3

[0045] A Janus-like bifunctional nanofiber, the preparation method of which comprises the following steps:

[0046] Polyvinyl alcohol was dissolved in dimethylformamide under continuous magnetic stirring at 70°C for 12 hours to obtain a 5% mass fraction solution A; polyvinyl alcohol, polymethyl methacrylate, and iron-based metal organic framework were dissolved in dimethylformamide at a mass ratio of 1:5:5 under continuous magnetic stirring at 80°C for 12 hours to obtain a 5% mass fraction solution B.

[0047] Solution A was used as the shell solution and solution B as the core solution, respectively, and added into a 25 ml syringe, with injection speeds of 3 ml / h and 3 ml / h, respectively, and the spinning voltage was 30 kV, the distance between the spinneret and the receiver was 40 cm, the receiver speed was 100 rpm, the temperature was 15 ° C, and the humidity was 40% for spinning parameters to obtain a core-shell structure polymer fiber precursor. The fiber was dried in a vacuum oven at 60 ° C for 12 hours.

[0048] 1.2mmol of cobalt nitrate and 1.8mmol of sodium citrate were added to 40ml of deionized water, and magnetic stirring was continued at room temperature for 30min to obtain solution C; the stirring speed of solution C was adjusted to 100rpm, and the core-shell structure polymer fiber cut into a certain size was placed in solution C and soaked for 30min; 0.8mmol of potassium ferrocyanide was added to 40ml of deionized water, and magnetic stirring was continued at room temperature for 30min to obtain solution D; solution D was slowly added to solution C and stirred for 4h, and then allowed to stand for 24h. The fiber was washed three times with ethanol and dried in a vacuum oven at 60℃ for 12h.

[0049] The temperature was first raised to 280°C in an air atmosphere at a heating rate of 10°C / min and maintained for 2 hours, and then raised to 1500°C in a mixed atmosphere of nitrogen and hydrogen at a heating rate of 10°C / min and maintained for 2 hours, and then cooled to room temperature with the furnace to obtain a core layer of porous nanorods derived from an iron metal organic framework, a shell layer of carbon nanofibers, and an outer layer of cubic cobalt-iron-based Prussian blue-derived Janus-structured bifunctional nanofibers.

[0050] Example 4

[0051] A Janus-like bifunctional nanofiber, the preparation method of which comprises the following steps:

[0052] Polyacrylonitrile was dissolved in dimethyl sulfoxide under continuous magnetic stirring at 80°C for 12 hours to obtain a 20% mass fraction solution A; polyacrylonitrile, polystyrene and nickel sulfide were dissolved in dimethyl sulfoxide at a mass ratio of 1:5:0.1 under continuous magnetic stirring at 80°C for 12 hours to obtain a 30% mass fraction solution B.

[0053] Solution A was used as the shell solution and solution B as the core solution, respectively, and added into a 25 ml syringe, the injection speed was 0.5 ml / h and 0.5 ml / h, respectively, the receiver speed was 50 rpm, the temperature was 25°C, the coagulation bath was a mixed solution of water and dimethyl sulfoxide, and the total traction ratio was 1 for wet spinning parameters to obtain a core-shell structure polymer fiber precursor. The fiber was dried in a vacuum oven at 60°C for 12 hours.

[0054] 1.2mmol of dimethylimidazole cobalt nitrate, 0.6mmol of ferric nitrate, 5mmol of ammonium fluoride and 10mmol of urea were added to 40ml of deionized water, and magnetic stirring was continued at room temperature for 30min to obtain solution C; the stirring speed of solution C was adjusted to 100rpm, and the core-shell structure polymer fiber cut into a certain size was placed in solution C and soaked for 30min; the fiber and solution were poured into a reactor and reacted at 130℃ for 8h. The fiber was washed three times with ethanol and dried in a vacuum oven at 60℃ for 12h. The dried fiber was placed in 40ml of aqueous solution containing 130mmol of sodium sulfide and reacted at 120℃ for 4h. The fiber was then washed three times with ethanol and dried in a vacuum oven at 60℃ for 12h.

[0055] The temperature was first raised to 250°C in an air atmosphere at a heating rate of 5°C / min and maintained for 2 hours, then raised to 500°C in a nitrogen atmosphere at a heating rate of 5°C / min and maintained for 4 hours, and then cooled to room temperature with the furnace to obtain a porous nanorod modified with nickel sulfide as the core layer, carbon nanofibers as the shell layer, and Janus-structured bifunctional nanofibers derived from flaky cobalt-iron-based metal sulfides as the outer layer.

[0056] Example 5

[0057] A Janus-like bifunctional nanofiber, the preparation method of which comprises the following steps:

[0058] Polyacrylonitrile was dissolved in dimethylacetamide under continuous magnetic stirring at 80°C for 12 h to obtain a solution A with a mass fraction of 12%. Polyacrylonitrile, polystyrene and iron selenide were dissolved in dimethylacetamide at a mass ratio of 2:2:1 under continuous magnetic stirring at 80°C for 12 h to obtain a solution B with a mass fraction of 15%.

[0059] Solution A was used as the shell solution and solution B as the core solution, respectively, and added into a 25 ml syringe, the injection speed was 1.4 ml / h and 0.7 ml / h, respectively, the receiver speed was 500 rpm, the temperature was 25°C, the coagulation bath was a mixed solution of water and dimethylacetamide, and the total traction ratio was 20 for wet spinning parameters to obtain a core-shell structure polymer fiber precursor. The fiber was dried in a vacuum oven at 60°C for 12 hours.

[0060] 1.2mmol of dimethylimidazole cobalt nitrate, 0.6mmol of ferric nitrate, 5mmol of ammonium fluoride and 10mmol of urea were added to 40ml of deionized water, and magnetic stirring was continued at room temperature for 30min to obtain solution C; the stirring speed of solution C was adjusted to 100rpm, and the core-shell structure polymer fiber cut into a certain size was placed in solution C and soaked for 30min; the fiber and solution were poured into a reactor and reacted at 130℃ for 8h. The fiber was washed three times with ethanol and dried in a vacuum oven at 60℃ for 12h. The dried fiber was placed in 40ml of 10mmol sodium selenide aqueous solution at 120℃ for 4h. The fiber was then washed three times with ethanol and dried in a vacuum oven at 60℃ for 12h.

[0061] The temperature was first raised to 250°C in an air atmosphere at a heating rate of 1°C / min and maintained for 2 hours, then raised to 800°C in an argon atmosphere at a heating rate of 1°C / min and maintained for 2 hours, and then cooled to room temperature with the furnace to obtain a porous nanorod modified with iron selenide as the core layer, carbon nanofibers as the shell layer, and Janus-like bifunctional nanofibers modified with flaky cobalt iron selenide as the outer layer.

[0062] Example 6

[0063] A Janus-like bifunctional nanofiber, the preparation method of which comprises the following steps:

[0064] Under continuous magnetic stirring at 80°C for 12 hours, polyacrylonitrile was dissolved in a mixed solution of dimethylformamide and 1-dodecyl-3-methylimidazole chloride (mass ratio 99:1) to obtain a solution A with a mass fraction of 11%. Under continuous magnetic stirring at 80°C for 12 hours, polyacrylonitrile, polymethyl methacrylate and ferrosoferric oxide nanoparticles were dissolved in dimethylformamide at a mass ratio of 1:3:1 to obtain a solution B with a mass fraction of 12%.

[0065] Solution A was used as the shell solution and solution B as the core solution, respectively, and added into a 25 ml syringe, with injection speeds of 1.5 ml / h and 0.7 ml / h, respectively, and the receiver speed was 500 rpm, the temperature was 25°C, the humidity was 40%, and the total traction ratio was 20. Dry spinning parameters were used to spin the core-shell structure polymer fiber precursor. The fiber was dried in a vacuum oven at 60°C for 12 hours.

[0066] 20 mmol of zinc acetate was added to 40 ml of ethanol, and the solution C was obtained by continuous magnetic stirring at room temperature for 30 min. The stirring speed of solution C was adjusted to 100 rpm, and 0.55 mmol of triethylamine was added dropwise to solution C. The core-shell polymer fiber cut into a certain size was placed in solution C and soaked at 100°C for 12 h. The fiber was washed three times with ethanol and dried in a vacuum oven at 60°C for 12 h.

[0067] The temperature was first raised to 250°C in an air atmosphere at a heating rate of 5°C / min and maintained for 2 hours, then raised to 800°C in a nitrogen atmosphere at a heating rate of 5°C / min and maintained for 2 hours, and then cooled to room temperature with the furnace to obtain a Janus-structured bifunctional nanofiber with a core layer of porous nanorods modified with ferroferric oxide, a shell layer of carbon nanofibers, and an outer layer of a cubic metal-organic framework modified with cobalt metal.

[0068] In summary, the embodiments of the present invention provide a method for preparing Janus-like bifunctional nanofibers by coaxial spinning and in-situ growth technology. The preparation method is simple and has a large fiber yield. The prepared nanofibers have a Janus structure and can be used in fields such as electrocatalysis, electromagnetic shielding and sensing.

[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing Janus-like bifunctional nanofibers, It is characterized in that The following steps are involved: (1) mixing and dissolving a high carbon yield polymer I, a pyrolysis polymer, a functional material, and a solvent I to obtain a first spinning solution; (2) mixing and dissolving the high carbon yield polymer II and the solvent II to obtain a second spinning solution; (3) using the first spinning solution as the inner solution and the second spinning solution as the outer solution, and spinning by coaxial spinning to obtain a core-shell structure polymer fiber membrane precursor; (4) placing the core-shell structure polymer fiber membrane precursor into the configured growth solution and immersing it to obtain Janus-like bifunctional polymer nanofibers; (5) The Janus-like bifunctional polymer nanofibers are calcined and carbonized to obtain Janus-like bifunctional nanocarbon fibers.

2. The method for preparing the Janus-like bifunctional nanofiber according to claim 1, It is characterized in that The functional material is one or more of functional salts, metal organic frameworks, Prussian blue-like compounds, hydroxides, oxides, sulfides and selenides; the functional salts are nitrates, chlorides, sulfates, acetates or acetylacetonates; the pyrolytic polymer is polymethyl methacrylate and / or polystyrene.

3. The method for preparing the Janus-like bifunctional nanofiber according to claim 2, It is characterized in that The high carbon yield polymer I and high carbon yield polymer II are respectively selected from one or more of polyacrylonitrile, polyvinyl pyrrolidone and polyvinyl alcohol; the solvent I and solvent II are respectively selected from one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide and ionic liquid.

4. The method for preparing the Janus-like bifunctional nanofiber according to claim 3, It is characterized in that The mass ratio of the high carbon yield polymer I, the pyrolysis polymer and the functional material is 1:(1-5):(0.1-5), the total concentration of the solute in the first spinning solution is 5-30wt%; the concentration of the high carbon yield polymer II in the second spinning solution is 5-30wt%.

5. The method for preparing the Janus-like bifunctional nanofiber according to claim 1, It is characterized in that The coaxial spinning is coaxial electrostatic spinning, coaxial wet spinning or coaxial dry spinning.

6. The method for preparing the Janus-like bifunctional nanofiber according to claim 5, It is characterized in that The coaxial spinning is coaxial electrospinning, and the process parameters of the coaxial electrospinning are: voltage of 8-30 kV, receiving distance of 10-40 cm, core layer solution injection speed of 0.5-3 ml / h, shell layer solution injection speed of 0.5-3 ml / h.

7. The method for preparing the Janus-like bifunctional nanofiber according to claim 1, It is characterized in that The growth solution is a precursor solution capable of in-situ growing a metal organic framework, a Prussian blue-like substance, a hydroxide, an oxide, a sulfide or a selenide on the fiber surface.

8. The method for preparing the Janus-like bifunctional nanofiber according to claim 7, It is characterized in that The soaking method is one or more of standing, stirring and ultrasound; the soaking time is 2-24 hours, and the soaking temperature is 0-150°C.

9. The method for preparing the Janus-like bifunctional nanofiber according to claim 1, It is characterized in that The calcination and carbonization steps are: first pre-oxidation at 150-280° C. for 1-3 hours, and then carbonization at 600-1500° C. for 1-4 hours.

10. A Janus-like bifunctional nanofiber prepared by the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Core-shell structure covalent organic framework / carbon nanotube fiber, preparation method and application thereof

    CN122147574A

  • Preparation method of hydrophobic conductive fiber and application of hydrophobic conductive fiber in antistatic suede material