Hydrogel optical fiber probe and preparation method and application thereof

By using a combination of hydrogel materials and silica microspheres to form a porous structure of optical fiber probes, the existing problems of complicated preparation of optical fiber probes and reliance on signal demodulation equipment are solved, achieving portability and flexibility, and supporting naked-eye observation. and diverse applications.

CN118812909APending Publication Date: 2024-10-22HUAQIAO UNIVERSITY
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410851692.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing fiber optic probes require tedious fiber processing and functional material modification during the preparation process, and rely on expensive signal demodulation equipment, which cannot meet the portability and comfort requirements for human body sign monitoring.

Method used

Optical fiber probes with porous structures are prepared using hydrogel materials. By combining polyethylene glycol diacrylate, alginic acid, polymethyl methacrylate and other hydrogels with silica microspheres, a hexagonally stacked three-dimensional order is formed. The porous structure enables sensing with intuitive color output without the need for signal demodulation equipment.

Benefits of technology

It realizes signal detection without signal demodulation equipment, supports naked eye observation, is suitable for human body sign monitoring, has flexibility and adjustable optical performance, and adapts to different application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812909A_ABST
    Figure CN118812909A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of optical fibers, and particularly relates to a hydrogel optical fiber probe and a preparation method and application thereof.The hydrogel optical fiber probe is made of one or more of polyethylene glycol diacrylate, alginic acid, polymethyl methacrylate, polyethylene glycol and polylactic acid-glycolic acid copolymer; the hydrogel optical fiber probe has a porous structure, and the porous structure is a hexagonal stacked three-dimensional ordered porous structure. The hydrogel optical fiber probe provided by the invention does not need signal demodulation equipment, and can realize visual color output, thereby supporting naked eye signal observation and expanding the application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical fibers, and in particular relates to a hydrogel optical fiber probe and a preparation method and application thereof. Background Art

[0002] In fiber optic sensors, fiber optic probes, as core devices, not only need to sense the object being measured, but also need to support the transmission of excitation light and signal light. Their performance directly determines the performance of the sensor, so their design and preparation are crucial.

[0003] Among the existing methods for preparing optical fiber probes, one is to modify the surface of quartz optical fiber with functional materials (such as organic fluorescent dyes, quantum dots and upconversion microspheres for fluorescence sensing; or gold or silver nanoparticles for surface plasmon resonance (SPR) sensing). However, quartz optical fiber probes often require cumbersome optical fiber processing and functional material modification steps, and all probes are difficult to reuse. In addition, such sensors all require the use of photodetectors or spectrometers to demodulate the signal. Another method for preparing optical fiber probes is to introduce microstructures into the optical fiber (such as etching a one-dimensional periodic structure in a quartz optical fiber to form a fiber Bragg grating) to achieve sensing. Although this method avoids the complex modification process of the functional materials of the optical fiber probe, the probe itself is difficult to prepare and the cost is high, and expensive equipment such as spectrometers are still required to demodulate the signal, so it cannot meet the portability and comfort requirements of human vital signs monitoring.

[0004] Hydrogel materials have excellent physical and chemical properties, and their large mesh structure can be used for biochemical detection. The flexibility, biocompatibility and low toxicity of hydrogel materials can be used for human vital signs monitoring; in addition, the rich variety of hydrogel materials ensures the diversity of their choices. However, existing hydrogel fiber optic probes still imitate the conventional "core-cladding" structure of traditional quartz optical fibers. Although they can also achieve sensing by embedding functional materials or causing changes in light intensity through deformation, like traditional optical fibers, they still rely on signal demodulation equipment, resulting in limited applications. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a hydrogel optical fiber probe and its preparation method and application. The hydrogel optical fiber probe provided by the present invention does not need to rely on signal demodulation equipment, can achieve intuitive color output, and thus supports naked eye observation of signals.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a hydrogel optical fiber probe, wherein the material of the hydrogel optical fiber probe includes one or more of polyethylene glycol diacrylate hydrogel, alginate hydrogel, polymethyl methacrylate hydrogel, polyethylene glycol hydrogel and polylactic acid-glycolic acid copolymer hydrogel;

[0008] The hydrogel optical fiber probe has a porous structure, and the porous structure is a three-dimensional ordered porous structure of hexagonal stacking.

[0009] Preferably, a waveguide vacancy structure is also included.

[0010] Preferably, the pore size of the porous structure is 120-250 nm.

[0011] Preferably, the number of the waveguide vacancy structures is ≥1.

[0012] The present invention also provides a method for preparing the hydrogel optical fiber probe described above, comprising the following steps:

[0013] dispersing a hydrogel monomer and a ketone photoinitiator into an alcohol solvent to obtain a hydrogel precursor solution;

[0014] Mixing the hydrogel precursor solution and the suspension of silica microspheres to obtain a silica / hydrogel microstructure solution;

[0015] After injection molding the silica / hydrogel microstructure solution, photocuring is performed to obtain a hydrogel solid optical fiber;

[0016] The hydrogel solid optical fiber is mixed with a hydrofluoric acid solution, and the silica microspheres are corroded and removed to obtain the hydrogel optical fiber probe; the hydrogel monomer includes one or more of polyethylene glycol diacrylate, alginate, polymethyl methacrylate, polyethylene glycol and polylactic acid-glycolic acid copolymer.

[0017] The present invention also provides a method for preparing the hydrogel optical fiber probe described above, comprising the following steps:

[0018] dispersing a hydrogel monomer and a ketone photoinitiator into an alcohol solvent to obtain a hydrogel precursor solution;

[0019] Mixing the hydrogel precursor solution and the suspension of silica microspheres to obtain a silica / hydrogel microstructure solution;

[0020] Injection molding the silica / hydrogel microstructure solution, then vertically embedding a quartz optical fiber into the liquid surface on one side of the silica / hydrogel microstructure solution, and performing photocuring to obtain a hydrogel solid optical fiber;

[0021] The hydrogel solid optical fiber is mixed with a hydrofluoric acid solution, and the silica microspheres and the quartz optical fiber are corroded and removed to obtain the hydrogel optical fiber probe; the hydrogel monomer includes one or more of polyethylene glycol diacrylate, alginate, polymethyl methacrylate, polyethylene glycol and polylactic acid-glycolic acid copolymer.

[0022] Preferably, the volume ratio of the hydrogel monomer, ketone photoinitiator and alcohol solvent is (100-140):(5-7):(150-190).

[0023] Preferably, the concentration of the hydrofluoric acid solution is 4-6 wt.%.

[0024] Preferably, the conditions for the photocuring are: the wavelength of ultraviolet light is 365-405 nm, and the light intensity is 12-30 cd / cm 2 , time is 3 to 10 minutes.

[0025] The present invention also provides the use of the hydrogel optical fiber probe described above or the hydrogel optical fiber probe prepared by the preparation method described above in detecting solutions of different concentrations; the solution includes an ethanol solution or a sodium chloride solution.

[0026] The present invention provides a hydrogel optical fiber probe, wherein the material of the hydrogel optical fiber probe includes one or more of polyethylene glycol diacrylate hydrogel, alginate hydrogel, polymethyl methacrylate hydrogel, polyethylene glycol hydrogel and polylactic acid-glycolic acid copolymer hydrogel; the hydrogel optical fiber probe has a porous structure, and the porous structure is a three-dimensional ordered porous structure of hexagonal stacking. When used, the hydrogel optical fiber probe provided by the present invention is directly placed in solutions with different refractive indices. After the solution enters the hole, its light modulation wavelength will change, that is, the color of the probe will be changed. Solutions with different refractive indices will make the probe produce different colors, thereby realizing naked eye observable signals. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of injection molding during the preparation of a quasi-periodic structure hydrogel optical fiber probe in Example 1;

[0028] Figure 2 Schematic diagram of etching and removing silica microspheres during the preparation of the quasi-periodic structure hydrogel optical fiber probe in Example 1;

[0029] Figure 3 Schematic diagram of the preparation of the waveguide type linear defect hydrogel optical fiber probe in Example 2;

[0030] Figure 4 Schematic diagram of the waveguide type linear defect hydrogel optical fiber probe in Example 2;

[0031] Figure 5 Schematic diagram of the preparation of the multi-defect three-dimensional microstructure hydrogel optical fiber probe in Example 3;

[0032] Figure 6 Schematic diagram of the multi-defect three-dimensional microstructure hydrogel optical fiber probe in Example 3. DETAILED DESCRIPTION

[0033] The present invention provides a hydrogel optical fiber probe, wherein the material of the hydrogel optical fiber probe includes one or more of polyethylene glycol diacrylate hydrogel, alginate hydrogel, polymethyl methacrylate hydrogel, polyethylene glycol hydrogel and polylactic acid-glycolic acid copolymer hydrogel;

[0034] The hydrogel optical fiber probe has a porous structure, and the porous structure is a three-dimensional ordered porous structure of hexagonal stacking.

[0035] In the present invention, the material of the hydrogel optical fiber probe includes one or more of polyethylene glycol diacrylate hydrogel, alginate hydrogel, polymethyl methacrylate hydrogel, polyethylene glycol hydrogel and polylactic acid-glycolic acid copolymer hydrogel, preferably polyethylene glycol diacrylate.

[0036] In the present invention, the hydrogel optical fiber probe has a porous structure, and the porous structure is a three-dimensional ordered porous structure of hexagonal stacking. In the present invention, the pore size of the porous structure is preferably 120-250 nm.

[0037] In the present invention, the hydrogel optical fiber probe preferably further comprises a waveguide vacancy structure. In the present invention, the number of the waveguide vacancy structure is ≥1, preferably 1-3.

[0038] In the present invention, the hydrogel optical fiber probe preferably further comprises a plastic optical fiber; the plastic optical fiber is located at one end of the hydrogel optical fiber probe. In the present invention, the plastic optical fiber comprises a core and a sheath. The material of the core is preferably one or more of polystyrene (PS), fluorinated polymethacrylate, polymethyl methacrylate (PMMA) and polyvinyl chloride (PVC), more preferably polymethyl methacrylate (PMMA); the diameter of the core is preferably 200 μm; the material of the sheath is preferably polymethacrylate, fluororesin or silicone resin, more preferably fluororesin; the thickness of the sheath is preferably 20 μm.

[0039] In the present invention, the hydrogel optical fiber probe provided by the present invention has flexibility in structural design and controllability of optical properties. For example, the size and arrangement of the hydrogel material and structure, silica microspheres and quartz optical fibers can be flexibly controlled to change the light-controlled mode field distribution and adapt to different application requirements.

[0040] The present invention also provides a method for preparing the hydrogel optical fiber probe described above, comprising the following steps:

[0041] dispersing a hydrogel monomer and a ketone photoinitiator into an alcohol solvent to obtain a hydrogel precursor solution;

[0042] Mixing the hydrogel precursor solution and the suspension of silica microspheres to obtain a silica / hydrogel microstructure solution;

[0043] After injection molding the silica / hydrogel microstructure solution, photocuring is performed to obtain a hydrogel solid optical fiber;

[0044] The hydrogel solid optical fiber is mixed with a hydrofluoric acid solution, and the silica microspheres are corroded and removed to obtain the hydrogel optical fiber probe.

[0045] The invention disperses hydrogel monomers and ketone photoinitiators into alcohol solvents to obtain a hydrogel precursor solution.

[0046] In the present invention, the hydrogel monomer includes one or more of polyethylene glycol diacrylate, alginic acid, polymethyl methacrylate, polyethylene glycol and polylactic acid-glycolic acid copolymer, more preferably polyethylene glycol diacrylate. In the present invention, the ketone photoinitiator preferably includes 2-hydroxy-2-methyl-1-phenyl-1-propanone and / or 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone. In the present invention, the particle size of the silica microspheres is preferably 120 to 250 nm, more preferably 150 to 200 nm. In the present invention, the alcohol solvent preferably includes an ethanol solution, and the concentration of the ethanol solution is preferably 98wt.%.

[0047] In the present invention, the volume ratio of the hydrogel monomer, ketone photoinitiator and alcohol solvent is preferably (100-140):(5-7):(150-190), and more preferably (100-130):6:(150-160).

[0048] After obtaining the hydrogel precursor solution, the present invention mixes the hydrogel precursor solution with a suspension of silica microspheres to obtain a silica / hydrogel microstructure solution.

[0049] In the present invention, the suspension of silica microspheres comprises silica microspheres and ethanol solution; the concentration of the ethanol solution is preferably 98wt.%; the volume ratio of the mass of silica microspheres in the suspension of silica microspheres to the ethanol solution is preferably 0.5-1.5g:8-10mL, more preferably 0.5-1.5g:8.5mL.

[0050] In the present invention, the mixing method is preferably ultrasonic mixing, the power of the ultrasonic mixing is preferably 50 W, and the time is preferably 15 to 20 minutes.

[0051] In the present invention, ultrasonic mixing can achieve degassing of the hydrogel precursor solution and dispersion of silica microspheres in the hydrogel precursor solution.

[0052] After obtaining the silica / hydrogel microstructure solution, the present invention performs injection molding on the silica / hydrogel microstructure solution and then performs photocuring to obtain a hydrogel solid optical fiber.

[0053] In the present invention, the injection mold body is preferably formed by injecting the silica / hydrogel microstructure solution into a silicone tube mold.

[0054] In the present invention, the conditions for photocuring are: the wavelength of ultraviolet light is preferably 365-405 nm, more preferably 370-400 nm, and the light intensity is preferably 12-30 cd / cm 2 , more preferably 15 to 20 cd / cm 2 The time is preferably 3 to 10 minutes, more preferably 5 to 8 minutes.

[0055] In the present invention, the photocuring can achieve polymerization of the hydrogel monomers under the conditions of ketone photoinitiator and light to obtain the hydrogel.

[0056] After obtaining the hydrogel solid optical fiber, the present invention mixes the hydrogel solid optical fiber with a hydrofluoric acid solution, and removes the silica microspheres by etching to obtain the hydrogel optical fiber probe.

[0057] In the present invention, the concentration of the hydrofluoric acid solution is preferably 4 to 6 wt.%.

[0058] In the present invention, the preparation of the hydrogel precursor solution and the silica / hydrogel microstructure solution are the same as above and will not be described in detail.

[0059] In the present invention, when the hydrogel optical fiber probe further includes a plastic optical fiber, it is preferred that the silica / hydrogel microstructure solution and the plastic optical fiber are combined and then photocured.

[0060] In the present invention, the combination of the silica / hydrogel microstructure solution and the plastic optical fiber is preferably: the silica / hydrogel microstructure solution is injected into a silicone tube mold for molding, and then one end of the plastic optical fiber is inserted into the silica / hydrogel microstructure solution in the silicone tube mold.

[0061] In the present invention, when the hydrogel optical fiber probe further includes a waveguide vacancy structure, the preparation method preferably includes the following steps:

[0062] dispersing a hydrogel monomer and a ketone photoinitiator into an alcohol solvent to obtain a hydrogel precursor solution;

[0063] Mixing the hydrogel precursor solution and the suspension of silica microspheres to obtain a silica / hydrogel microstructure solution;

[0064] Injection molding the silica / hydrogel microstructure solution, then vertically embedding a quartz optical fiber into the liquid surface on one side of the silica / hydrogel microstructure solution, and performing photocuring to obtain a hydrogel solid optical fiber;

[0065] The hydrogel solid optical fiber is mixed with a hydrofluoric acid solution, and the silica microspheres and the quartz optical fiber are corroded and removed to obtain the hydrogel optical fiber probe.

[0066] In the present invention, the preparation of the hydrogel precursor solution and the silica / hydrogel microstructure solution is preferably the same as described above, which will not be repeated here.

[0067] After obtaining the silica / hydrogel microstructure solution, the present invention injects the silica / hydrogel microstructure solution into a mold, then vertically embeds a quartz optical fiber into the liquid surface on one side of the silica / hydrogel microstructure solution, and performs photocuring to obtain a hydrogel solid optical fiber.

[0068] In the present invention, the quartz optical fiber preferably includes a core and a sheath; the materials of the core and the sheath are preferably quartz; and the thickness of the sheath is preferably 20 μm.

[0069] In the present invention, the injection molding is preferably an injection silicone tube mold.

[0070] In the present invention, the operation and conditions of the photocuring are preferably the same as those described above and will not be described in detail.

[0071] After obtaining the hydrogel solid optical fiber, the present invention mixes the hydrogel solid optical fiber with a hydrofluoric acid solution, and removes the silica microspheres and the quartz optical fiber by corrosion to obtain the hydrogel optical fiber probe.

[0072] In the present invention, the concentration of the hydrofluoric acid solution is preferably the same as above, which will not be described in detail here.

[0073] In the present invention, when the number of the waveguide vacancy structures is greater than 1, the preparation of the hydrogel solid optical fiber is preferably as follows: the silica / hydrogel microstructure solution is injected into a silicone tube mold in batches for molding, and after each molding, a section of quartz optical fiber is inserted into the section of silica / hydrogel microstructure solution in the silicone tube mold for combination.

[0074] In the present invention, when the hydrogel optical fiber probe has a waveguide vacancy structure, the output of light with different resonant frequencies can be realized, thereby realizing distributed and multi-parameter sensing. By optimizing the defect structure, extremely low light transmission loss can also be achieved, thereby ensuring long-distance transmission of light, which can be used for in-situ analysis, in vivo detection and multi-point measurement.

[0075] In the present invention, when the hydrogel optical fiber probe preferably further comprises a plastic optical fiber, after the injection molding, it preferably further comprises: combining the plastic optical fiber with a silica / hydrogel microstructure solution.

[0076] The present invention also provides the use of the hydrogel optical fiber probe described above or the hydrogel optical fiber probe prepared by the preparation method described above in detecting solutions of different concentrations.

[0077] In the present invention, the solution preferably includes an ethanol solution or a sodium chloride solution.

[0078] In the present invention, the application analyzes the environmental water quality in real time by detecting the refractive index of the liquid, and reflects and detects the humidity change in the air in real time in humid areas.

[0079] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0080] Example 1

[0081] 1081.2 μL of polyethylene glycol diacrylate, 55.7 μL of 2-hydroxy-2-methyl-1-phenyl-1-propanone, and 1863.1 μL of 98 wt. % ethanol solution were mixed to obtain a hydrogel precursor solution.

[0082] 0.83 g of silica microspheres with a particle size of 200 nm and 8.5 mL of 98 wt.% ethanol solution were added to the above precursor solution, and after ultrasonic degassing and dispersion, a silica / hydrogel microstructure solution was formed.

[0083] A hollow silicone tube mold with an inner diameter of 3 mm and a length of 3 cm was fixed with a fixture, and the silica / hydrogel microstructure solution was injected into the hollow silicone tube mold with a syringe. A plastic optical fiber with a core and cladding diameter of 200 μm and 220 μm, respectively, was inserted into the silica / hydrogel microstructure solution in the central area of ​​the silicone tube mold. The above structure was placed under a 365 nm ultraviolet light source for 5 minutes for curing, and then the cured structure was pushed out of the silicone tube mold with deionized water to obtain a hydrogel solid optical fiber.

[0084] The hydrogel solid optical fiber was immersed in a 5wt.% hydrofluoric acid solution for etching for 5 hours. After the silica microspheres were completely etched, they were washed with deionized water to obtain a three-dimensional microstructure hydrogel optical fiber probe with an air hole structure, which was recorded as a quasi-periodic structure hydrogel optical fiber probe.

[0085] Figure 1 Schematic diagram of injection molding in the process of preparing the quasi-periodic structure hydrogel optical fiber probe in Example 1, wherein: 1-silicon dioxide / hydrogel microstructure solution; 2-silicone tube mold; 3-fixing fixture; 4-injector; 5-plastic optical fiber; 6-ultraviolet lamp; 7-hydrogel solid optical fiber; 8-hydrofluoric acid solution; 9-quasi-periodic structure hydrogel optical fiber probe 9; Figure 1 It can be seen that: the present invention fixes the silicone tube mold 2 on the fixing fixture 3, and uses the syringe 4 to inject the prepared silica / hydrogel microstructure solution 1 into the silicone tube mold 2; then, the plastic optical fiber 5 is inserted into the silica / hydrogel microstructure solution 1 in the transparent silicone tube mold 2, and photocured under the irradiation of the ultraviolet lamp 6 to obtain the hydrogel solid optical fiber 7.

[0086] Figure 2 Schematic diagram of etching and removing silica microspheres during the preparation of the quasi-periodic structure hydrogel optical fiber probe in Example 1. Figure 2 It can be seen that the prepared hydrogel solid optical fiber 7 is placed in a hydrofluoric acid solution 8, and the hydrofluoric acid solution 8 corrodes the silica microspheres into holes, thereby obtaining the quasi-periodic structure hydrogel optical fiber probe 9.

[0087] The hydrogel solid optical fiber is mixed with a hydrofluoric acid solution, and the silica microspheres are corroded and removed to obtain the hydrogel optical fiber probe.

[0088] Example 2

[0089] 1351.5 μL of polyethylene glycol diacrylate, 69.6 μL of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 1578.9 μL of 98 wt. % ethanol solution were mixed to prepare a hydrogel precursor solution.

[0090] 1.03 g of silica microspheres with a particle size of 200 nm and 8.5 mL of 98 wt.% ethanol solution were added to the above precursor solution, and after ultrasonic degassing and dispersion, a silica / hydrogel microstructure solution was formed.

[0091] A hollow silicone tube mold with an inner diameter of 3 mm and a length of 3 cm was fixed with a fixture, and the silica / hydrogel microstructure solution was injected into the hollow silicone tube mold with a syringe. A multimode quartz optical fiber with a length of 2.5 cm, a core diameter of 105 μm, and a cladding diameter of 125 μm was inserted into the silica / hydrogel microstructure solution in the central area of ​​the silicone tube mold. Then, a plastic optical fiber with a core diameter of 200 μm was inserted into the silica / hydrogel microstructure solution in the central area of ​​the silicone tube mold. The above structure was placed under a 365 nm ultraviolet light source for 5 minutes for curing, and the cured structure was pushed out of the silicone tube mold with deionized water to obtain a hydrogel solid optical fiber.

[0092] The hydrogel solid optical fiber was immersed in a 5wt.% hydrofluoric acid solution for 10 hours for corrosion. After the silica microspheres and multimode quartz optical fiber were completely corroded, they were washed with deionized water to obtain the hydrogel optical fiber probe, which was recorded as a waveguide linear defect hydrogel optical fiber probe.

[0093] Figure 3 is a schematic diagram of the preparation of the waveguide type linear defect hydrogel optical fiber probe in Example 2; Figure 3 It can be seen that in order to obtain a hydrogel solid optical fiber with a waveguide vacancy structure, the quartz optical fiber is combined with a silica / hydrogel microstructure solution and then corroded and removed.

[0094] Figure 4 is a schematic diagram of the waveguide type linear defect hydrogel optical fiber probe in Example 2, from Figure 4 It can be seen that after etching and removing the quartz optical fiber, a hydrogel optical fiber probe with waveguide defects is obtained. The probe can realize broadband wavelength white light input, while narrowband wavelength light is output through the waveguide wire defect structure, with high transmission efficiency.

[0095] Example 3

[0096] 1263 μL of polyethylene glycol diacrylate, 69.6 μL of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 1578.9 μL of 98 wt. % ethanol solution were mixed to prepare a hydrogel precursor solution.

[0097] 1.21 g of silica microspheres with a particle size of 200 nm and 8.5 mL of 98 wt.% ethanol solution were added to the above precursor solution, and after ultrasonic degassing and dispersion, a silica / hydrogel microstructure solution was formed.

[0098] A hollow silicone tube mold with an inner diameter of 2 mm and a length of 5 cm was fixed with a fixing fixture. First, 200 μL of silica / hydrogel microstructure solution was injected into the hollow silicone tube mold with a syringe. Then, a multimode quartz optical fiber with a length of 0.5 cm, a core diameter of 105 μm, and a cladding diameter of 125 μm was inserted into the silica / hydrogel microstructure solution in the center area of ​​the silicone tube mold.

[0099] Afterwards, 600 μL of silica / hydrogel microstructure solution was injected into the hollow silicone tube mold with a syringe, and a multimode quartz optical fiber with a length of 1 cm, a core diameter of 105 μm, and a cladding diameter of 125 μm was inserted into the silica / hydrogel microstructure solution in the center area of ​​the silicone tube mold; after that, the remaining area was injected with silica / hydrogel microstructure solution. Then, a plastic optical fiber with a core diameter of 200 μm was inserted into the silica / hydrogel microstructure solution in the center area of ​​the silicone tube mold. The above structure was placed under a 365 nm ultraviolet light source for 5 minutes for curing, and the cured structure was pushed out of the silicone tube mold with deionized water to obtain a hydrogel solid optical fiber.

[0100] The hydrogel solid optical fiber was immersed in a 5wt.% hydrofluoric acid solution for 10 hours for corrosion. After the silica microspheres and multimode quartz optical fiber were completely corroded, they were washed with deionized water to obtain the hydrogel optical fiber probe, which was recorded as a multi-defect hydrogel optical fiber probe.

[0101] Figure 5 is a schematic diagram of the preparation of the multi-defect three-dimensional microstructure hydrogel optical fiber probe in Example 3; Figure 5 It can be seen that in order to obtain a hydrogel solid optical fiber with a multi-segment waveguide vacancy structure, the silica / hydrogel microstructure solution is injected twice; after each molding, it is combined with a quartz optical fiber.

[0102] Figure 6 is a schematic diagram of a multi-defect three-dimensional microstructure hydrogel optical fiber probe in Example 3, Figure 6 It can be seen that the multi-defect three-dimensional microstructure hydrogel optical fiber probe can set different waveguide defects at different positions, have different resonant wavelengths, and realize distributed sensing.

[0103] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A hydrogel optical fiber probe, characterized in that: The material of the hydrogel optical fiber probe includes one or more of polyethylene glycol diacrylate hydrogel, alginate hydrogel, polymethyl methacrylate hydrogel, polyethylene glycol hydrogel and polylactic acid-glycolic acid copolymer hydrogel; The hydrogel optical fiber probe has a porous structure, and the porous structure is a three-dimensional ordered porous structure of hexagonal stacking.

2. The hydrogel optical fiber probe according to claim 1, characterized in that: Also included are waveguide vacancy structures.

3. The hydrogel optical fiber probe according to claim 1 or 2, characterized in that: The pore diameter of the porous structure is 120-250 nm.

4. The hydrogel optical fiber probe according to claim 2, characterized in that: The number of the waveguide vacancy structures is ≥1.

5. The method for preparing the hydrogel optical fiber probe according to claim 1, characterized in that: The following steps are involved: dispersing a hydrogel monomer and a ketone photoinitiator into an alcohol solvent to obtain a hydrogel precursor solution; Mixing the hydrogel precursor solution and the suspension of silica microspheres to obtain a silica / hydrogel microstructure solution; After injection molding the silica / hydrogel microstructure solution, photocuring is performed to obtain a hydrogel solid optical fiber; The hydrogel solid optical fiber is mixed with a hydrofluoric acid solution, and the silica microspheres are corroded and removed to obtain the hydrogel optical fiber probe; the hydrogel monomer includes one or more of polyethylene glycol diacrylate, alginate, polymethyl methacrylate, polyethylene glycol and polylactic acid-glycolic acid copolymer.

6. The method for preparing the hydrogel optical fiber probe according to claim 2, characterized in that: The following steps are involved: dispersing a hydrogel monomer and a ketone photoinitiator into an alcohol solvent to obtain a hydrogel precursor solution; Mixing the hydrogel precursor solution and the suspension of silica microspheres to obtain a silica / hydrogel microstructure solution; Injection molding the silica / hydrogel microstructure solution, then vertically embedding a quartz optical fiber into the liquid surface on one side of the silica / hydrogel microstructure solution, and performing photocuring to obtain a hydrogel solid optical fiber; The hydrogel solid optical fiber is mixed with a hydrofluoric acid solution, and the silica microspheres and the quartz optical fiber are corroded and removed to obtain the hydrogel optical fiber probe; the hydrogel monomer includes one or more of polyethylene glycol diacrylate, alginate, polymethyl methacrylate, polyethylene glycol and polylactic acid-glycolic acid copolymer.

7. The preparation method according to claim 5 or 6, characterized in that: The volume ratio of the hydrogel monomer, the ketone photoinitiator and the alcohol solvent is (100-140):(5-7):(150-190).

8. The preparation method according to claim 5 or 6, characterized in that: The concentration of the hydrofluoric acid solution is 4-6 wt.%.

9. The preparation method according to claim 5 or 6, characterized in that: The conditions for the photocuring are: the wavelength of ultraviolet light is 365-405nm, and the light intensity is 12-30cd / cm 2 , time is 3 to 10 minutes.

10. Use of the hydrogel optical fiber probe according to any one of claims 1 to 4 or the hydrogel optical fiber probe prepared by the preparation method according to any one of claims 5 to 9 in detecting solutions of different concentrations; the solution comprises an ethanol solution or a sodium chloride solution.

Citation Information

Cited By

  • Optical fiber biosensor, flexible photonic crystal fiber and preparation method of flexible photonic crystal fiber

    CN120445992A

  • Fiber optic biosensor, flexible photonic crystal fiber and preparation method thereof

    CN120445992B

  • Organic-inorganic hybrid aerogel fiber as well as preparation method and application thereof

    CN122446365A