Composite anti-core-burning agent and application thereof

By using a porous silica-coated composite anti-burn core agent in the polyurethane sponge, the problems of aging and poor compatibility of the polyurethane sponge at high temperatures are solved, the core burn and organic volatilization are significantly improved, the product life is extended and the Antioxidant effect.

CN118812922AInactive Publication Date: 2024-10-22SHANGHAI PETROCHEM XINIER CHEM TECHCO
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410879953.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the production process of existing polyurethane sponges, due to long-term sustained high temperature, the chemical bonds of organic molecules are broken, generating active free radicals, which in turn accelerates aging and thermal degradation, affecting the appearance and service life of the product, and the combination of multiple antioxidants is compatible It has poor properties and is difficult to exert the expected antioxidant effect.

Method used

The composite anti-burning core agent uses porous silica coating antioxidants ST-1912, ST-5067, and ST-508T to form a stable combination state in the polyurethane sponge foaming system and utilize the pore size structure of porous silica. Slow release and adsorption of oxidation products improve the compatibility and antioxidant effect of antioxidants.

Benefits of technology

It significantly improves the core burning and organic volatilization phenomena of polyurethane sponge, extends the service life of the product, maintains good antioxidant effects in high temperature environments, and improves the overall application quality of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004924202090000091
    Figure BDA0004924202090000091
  • Figure BDA0004924202090000101
    Figure BDA0004924202090000101
Patent Text Reader

Abstract

The invention relates to the technical field of polyurethane oxidation resistance, and particularly discloses a composite anti-core-burning agent and application. The composite anti-core-burning agent is obtained by coating an antioxidant with porous silicon dioxide, and the preparation method comprises the following steps: S1, mixing hexadecyl trimethyl ammonium bromide, triethanolamine and distilled water, and stirring at 75-85 DEG C for 30-50 minutes to obtain a mixed solution; and S2, adding an antioxidant into the mixed solution, uniformly mixing, then adding tetraethoxysilane and ammonia water, reacting for 18-24 hours, centrifuging, washing and drying to obtain the product, the antioxidant is a mixture of at least any two of ST-1912, ST-5067 and ST-508T, and the antioxidant is a mixture of at least any two of the ST-1912, the ST-5067 and the The weight ratio of the antioxidant to the porous silicon dioxide is 1: (0.36-0.47). After the composite anti-core-burning agent disclosed by the invention is applied, various antioxidant components contained in the composite anti-core-burning agent can exert an excellent matching effect at a long-time continuous high temperature, so that the phenomena of core burning and organic matter volatilization of the polyurethane sponge can be obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polyurethane anti-oxidation, and more specifically, to a composite anti-core burning agent and its application. Background Art

[0002] Polyether polyol, referred to as polyether, is an organic polymer, mainly used to prepare soft, hard and semi-rigid polyurethane foam plastics. It is widely used in refrigerators, freezers, refrigerated trucks, insulation boards, pipe insulation, wall insulation, decorative coatings and other fields.

[0003] Polyurethane foaming is classified into hard foam, soft foam and semi-hard foam according to the process. In the production process of ordinary soft foam polyether, the addition of water causes high temperature in the center of the product. The long-term high temperature will break the chemical bonds of organic molecules and generate active free radicals. These free radicals can trigger a series of free radical chain reactions that will accelerate aging. Polyether will also be oxidized to generate peroxides, which will cause thermal degradation in the early stage of foam maturation, resulting in aging and yellowing, which will cause the sponge to burn and affect the appearance and service life. Therefore, antioxidants must be added when producing polyurethane materials to slow down the degradation rate of products during storage and processing, and improve their stability and service life.

[0004] In the preparation of polyurethane sponge, polyether polyol (and polyester polyol) and polyisocyanate are mainly used as the main raw materials, and auxiliary agents such as foaming agents, catalysts, foam stabilizers, and antioxidants are used in conjunction; among them, the commonly used polyurethane antioxidants include BHT, MB, AO-2246, etc. In actual application, multiple types of antioxidants are often used in combination.

[0005] Regarding the above-mentioned related technologies, the inventors believe that although the combined use of multiple antioxidants can improve the antioxidant performance to a certain extent, their combination and coordination with each other are poor, and their compatibility with ingredients such as polyether polyols (and polyester polyols) and polyisocyanates is poor. Especially under the influence of long-term continuous high temperature in the center of the product, it is difficult to exert the expected antioxidant effect.

[0006] Therefore, the core burning and organic volatilization of polyurethane sponge still need to be improved, and it is urgent to propose a solution to solve the above technical problems. Summary of the invention

[0007] In order to enable various combinations of antioxidants to exert excellent coordination effects under long-term continuous high temperature, thereby significantly improving the core burning and organic matter volatilization of polyurethane sponge, the present application provides a composite anti-core burning agent and its application.

[0008] In the first aspect, the present application provides a composite anti-core burning agent, which adopts the following technical solution: A composite anti-burning agent is obtained by coating an antioxidant with porous silica, and the preparation steps are as follows: S1. Mix cetyltrimethylammonium bromide, triethanolamine and distilled water, and stir at 75-85° C. for 30-50 min to obtain a mixed solution; S2, adding an antioxidant to the mixed solution, mixing evenly, then adding ethyl orthosilicate and ammonia water, reacting for 18-24 hours, centrifuging, washing, and drying to obtain; The antioxidant is a mixture of at least any two of ST-1912, ST-5067, and ST-508T; The weight ratio of the antioxidant to the porous silica is 1:(0.36-0.47).

[0009] By adopting the above technical scheme, the composite anti-burning agent is obtained by coating the antioxidant with porous silica, the antioxidant is a mixture of at least any two of ST-1912, ST-5067, and ST-508T, and the weight ratio of the antioxidant to the porous silica is 1: (0.36-0.47), so that the two can form a relatively stable binding state. Further, in the above preparation process, the antioxidant is present in the pore structure of the porous silica, so that the composite anti-burning agent has better compatibility with polyether polyols (and polyester polyols), polyisocyanates and other components in the foaming system of the polyurethane sponge; and, when the foaming process is affected by the long-term high temperature in the center of the product, the presence of porous silica can not only coordinate and protect the antioxidant, but also disperse and conduct the heat accumulated in the center, creating better conditions for the performance of various combinations of antioxidants. At the same time, the antioxidant in the porous silica can be slowly released during the foaming process of the polyurethane sponge, and combined with the adsorption of oxidation products by the porous silica after the antioxidant is released, the antioxidants in various combinations can show antioxidant effects. In summary, the excellent coordination effect of the porous silica on various antioxidants shows a synergistic effect, and the adaptability is outstanding under long-term high temperature, which can significantly improve the core burning and organic volatilization of the polyurethane sponge.

[0010] Preferably, the weight ratio of the antioxidant to the porous silica is 1:0.4.

[0011] By adopting the above technical scheme, during the application process of the composite anti-burning agent formed by combining the antioxidant and porous silica in the above weight ratio, the sustained release of the antioxidant and the adsorption of the oxidation products can be maintained in a better balance, which is more conducive to the full coordination effect of various combinations of antioxidants in a long-term continuous high temperature environment, so that the core burning and organic volatilization of the polyurethane sponge are relatively small, and the overall application quality of the composite anti-burning agent is better.

[0012] Preferably, the antioxidant is composed of the following components in parts by weight: ST-508T 5-20 copies; ST-1912 50-65 copies; ST-5067 25-40 servings.

[0013] By adopting the above technical scheme, the above types of antioxidants can meet the requirements of polyurethane sponge foaming applications after being used in the above dosage combinations, and the antioxidant effect brought about is also relatively comprehensive. In the process of preparing the composite anti-core burning agent, it can be stably loaded in the pore size of porous silica, and is not easy to migrate and precipitate under the influence of long-term continuous high temperature, so that the obtained composite anti-core burning agent can play a better corresponding technical effect in improving the core burning and organic volatilization of polyurethane sponge.

[0014] Preferably, the mass ratio of hexadecyltrimethylammonium bromide, triethanolamine and distilled water is (5-7):1:(380-420).

[0015] By adopting the above technical scheme, in the generation of silica, hexadecyltrimethylammonium bromide is dissolved in water, with its hydrophilic ammonium group facing the water and the hydrophobic alkyl long chain facing the inside to form rod-shaped micelles. After the subsequent addition of tetraethyl orthosilicate and ammonia water, the silicon source will be negatively charged, and the ammonium salt ions can adsorb the negatively charged silicon source on the surface of the rod-shaped micelles through the action of electrostatic attraction, and then the silicon source undergoes hydrolysis and condensation reaction to form porous silica. During the entire reaction process, the mass ratio of hexadecyltrimethylammonium bromide, triethanolamine and distilled water is (5-7):1:(380-420). After mixing in the above ratio, a more suitable reaction system can be built, which is conducive to the formation of a stable combination between the porous silica and the silica, thereby ensuring that the final composite anti-burning agent has better application quality.

[0016] Preferably, in step S2, the concentration of ethyl orthosilicate after addition is 0.5-1 mol / L.

[0017] By adopting the above technical scheme and selecting the above concentration of ethyl orthosilicate, it has a relatively moderate reaction rate during the reaction process, forming the polymerization degree and cross-linking degree of Si-O-Si, so that the porous silica not only has a stable structure, but also can form a stable load for the antioxidant, thereby ensuring that the final composite anti-core burning agent has a relatively excellent corresponding effect after application.

[0018] Preferably, in step S2, the concentration of ammonia water after addition is 0.9-1.5 mol / L.

[0019] By adopting the above technical scheme, the concentration of ammonia water is closely related to the particle size and pore structure of the porous silica. The selection of the above concentration range makes the pore structure of the porous silica richer, and shows better application effect on the sustained release of various combined antioxidants and the adsorption of oxidation products, thereby obtaining a composite anti-core agent of better quality.

[0020] Preferably, the composite anti-burning agent is obtained by coating an antioxidant with porous silica and then performing surface modification, and the preparation steps are as follows: (1) mixing hexadecyltrimethylammonium bromide, triethanolamine and distilled water, and stirring at 75-85° C. for 30-50 minutes to obtain a mixed solution; (2) adding an antioxidant to the mixed solution, mixing well, then adding ethyl orthosilicate and ammonia water, reacting for 18-24 hours, centrifuging, washing, and drying to obtain an intermediate product; (3) ultrasonically dispersing the intermediate product in a mixed solution of ethanol and deionized water, adjusting the pH to 4-5, adding a silane coupling agent, stirring at 45-55° C. for 2-3 hours, centrifuging, washing, and drying to obtain a pretreated intermediate product; (4) ultrasonically dispersing the pretreated intermediate product and the dispersant in a mixture of ethanol and ethyl acetate, then adding styrene monomer, emulsifying for 25-35 minutes, then heating to 60-70° C., adding an initiator, reacting at 55-65° C. for 6-8 hours, and washing and drying to obtain; The antioxidant is a mixture of at least any two of ST-1912, ST-5067, and ST-508T; The weight ratio of the antioxidant to the porous silica is 1:(0.36-0.47).

[0021] By adopting the above technical scheme, the surface of the obtained composite anti-burning agent in the treatment of step (3) and step (4) can be an inorganic-organic hybrid structure, which is easier to fully disperse and play a role in the polyurethane sponge foaming system; at the same time, the organic body on the surface of the composite anti-burning agent can stably regulate the release of multiple combined antioxidants under the influence of long-term high temperature in the center of the product, and enable the multiple combined antioxidants to fully cooperate with each other, thereby enabling the composite anti-burning agent to bring better improvement effects on the core burning and organic volatilization of the polyurethane sponge.

[0022] Preferably, the pre-treated intermediate product is 0.6-0.8% of the mass of the styrene monomer.

[0023] By adopting the above technical scheme and selecting the above ratios, the hybrid structure on the surface of the composite anti-burning agent is relatively stable. Under the premise of ensuring good dispersibility, various combinations of antioxidants can be stably released under long-term high temperature and exert a relatively excellent synergistic effect, thereby obtaining a composite anti-burning agent with better quality.

[0024] In the second aspect, the present application provides an application of a composite anti-core burning agent, using the following technical solution: The invention discloses an application of a composite anti-core burning agent. The composite anti-core burning agent is applied in the preparation of polyurethane sponge. The addition amount of the composite anti-core burning agent is 0.4-0.8wt%.

[0025] By adopting the above technical solution, during the foaming process of the polyurethane sponge, only the above-mentioned amount of the composite anti-core burning agent needs to be added, which can achieve a good application effect and meet the application requirements in improving the core burning and organic volatilization of the polyurethane sponge.

[0026] In summary, this application has the following beneficial effects: 1. The present application utilizes porous silica to exert an excellent synergistic effect on the coordination effect of multiple antioxidants, so that the composite anti-core burning agent not only exhibits excellent compatibility after application, but also can well cope with the heat accumulated in the center of the product, and promotes the coordination between each other through the slow-release antioxidant and the porous silica adsorption of oxidation products, thereby significantly improving the core burning and organic volatilization of the polyurethane sponge; 2. The present application forms an inorganic-organic hybrid structure on the surface of the composite anti-burning agent, which not only makes it easier for the composite anti-burning agent to be fully dispersed and exert its effect in the polyurethane sponge foaming system, but also can stably regulate the release of various combined antioxidants and enable the various combined antioxidants to fully cooperate with each other, thereby enabling the composite anti-burning agent to bring better improvement effects on the burning of the polyurethane sponge and the volatilization of organic matter. DETAILED DESCRIPTION

[0027] The present application is further described in detail below with reference to examples and comparative examples.

[0028] Unless otherwise specified, the raw materials used in the preparation examples and embodiments of the present application are commercially available. Example

[0029] Example 1 A composite anti-burning agent is obtained by coating an antioxidant with porous silica, wherein the weight ratio of the antioxidant to the porous silica is 1:0.4, and the components of the antioxidant and their corresponding weights are shown in Table 1, and the preparation steps are as follows: S1, cetyltrimethylammonium bromide, triethanolamine and distilled water are mixed, and stirred at 75-85° C. for 30-50 min (preferably at 80° C. for 40 min, with a stirring speed of 300 rpm) to obtain a mixed solution; S2. Add an antioxidant to the mixed solution, mix well, then add tetraethyl orthosilicate and ammonia water, react for 18-24 hours (preferably 20 hours in this embodiment), centrifuge (6000 rpm for 6 minutes), wash (wash 3 times with anhydrous ethanol), and dry (dry at 50° C. for 12 hours) to obtain.

[0030] Note: In the above steps, the mass ratio of hexadecyltrimethylammonium bromide, triethanolamine and distilled water is 6:1:400; the concentration of ethyl orthosilicate after addition is 0.75 mol / L; the concentration of ammonia water after addition is 1.2 mol / L.

[0031] Example 2-3 A composite anti-core burning agent, which is different from Example 1 in that the components of the antioxidant and their corresponding weights are shown in Table 1.

[0032] Table 1 Antioxidant components and their weight parts in Examples 1-3 (kg / part) raw material Example 1 Example 2 Example 3 ST-508T 12.5 5 20 ST-1912 57.5 50 65 ST-5067 32.5 25 40 Example 4 A composite anti-core burning agent, which is different from Example 1 in that the weight ratio of the antioxidant to the porous silica is 1:0.3.

[0033] Example 5 A composite anti-core burning agent, which is different from Example 1 in that the weight ratio of the antioxidant to the porous silica is 1:0.47.

[0034] Example 6 A composite anti-core burning agent, which is different from Example 1 in that the weight ratio of the antioxidant to the porous silica is 1:0.41.

[0035] Example 7 A composite anti-core burning agent is different from Example 1 in that the mass ratio of hexadecyltrimethylammonium bromide, triethanolamine and distilled water is 5:1:380.

[0036] Example 8 A composite anti-core burning agent is different from Example 1 in that the mass ratio of hexadecyltrimethylammonium bromide, triethanolamine and distilled water is 7:1:420.

[0037] Example 9 A composite anti-core burning agent, which is different from Example 1 in that, in step S2, the concentration of ethyl orthosilicate after addition is 0.5 mol / L.

[0038] Example 10 A composite anti-core burning agent, which is different from Example 1 in that, in step S2, the concentration of ethyl orthosilicate after addition is 1 mol / L.

[0039] Embodiment 11 A composite anti-core burning agent, which is different from Example 1 in that, in step S2, the concentration of ammonia water after addition is 0.9 mol / L.

[0040] Example 12 A composite anti-core burning agent, which is different from Example 1 in that, in step S2, the concentration of ammonia water after addition is 1.5 mol / L.

[0041] Example 13 A composite anti-core burning agent, which is different from Example 1 in that it is obtained by coating an antioxidant with porous silica and then performing surface modification, and the preparation steps are as follows: (1) mixing hexadecyltrimethylammonium bromide, triethanolamine and distilled water, stirring at 75-85° C. for 30-50 min (preferably at 80° C. for 40 min, at a stirring speed of 300 rpm) to obtain a mixed solution; (2) adding an antioxidant to the mixed solution, mixing well, then adding tetraethyl orthosilicate and ammonia water, reacting for 18-24 hours (preferably 20 hours in this embodiment), centrifuging (6000 rpm for 6 minutes), washing (washing with anhydrous ethanol 3 times), and drying (drying at 50° C. for 12 hours) to obtain an intermediate product; (3) ultrasonically dispersing the intermediate product in a mixed solution of ethanol and deionized water, adjusting the pH to 4.5, adding a silane coupling agent, stirring at 50° C. for 2.5 h, centrifuging (6000 rpm for 6 min), washing (washing with anhydrous ethanol 3 times), and drying (drying at 50° C. for 12 h) to obtain a pretreated intermediate product; (4) The pretreated intermediate product and the dispersant are ultrasonically dispersed in a mixture of ethanol and ethyl acetate in an amount of 10 times by weight, and then styrene monomer is added, emulsified for 30 minutes, and then the temperature is raised to 65° C., an initiator is added, and the mixture is reacted at 60° C. for 7 hours, and then washed (washed 3 times with anhydrous ethanol) and dried (dried at 40° C. for 8 hours) to obtain a product.

[0042] Note: In the above operation, the pretreatment intermediate product is 0.7% of the mass of the styrene monomer; the dispersant is polyvinyl pyrrolidone, and its dosage is 4% of the mass of the styrene monomer; the ethanol and ethyl acetate mixture is prepared by mixing ethanol and ethyl acetate in a volume ratio of 1:3; the initiator is benzoyl peroxide, which is 1.5% of the mass of the styrene monomer.

[0043] Embodiment 14 A composite anti-core burning agent, which is different from Example 13 in that step (3) and step (4) are specifically as follows: (3) ultrasonically dispersing the intermediate product in a mixed solution of ethanol and deionized water, adjusting the pH to 4, adding a silane coupling agent, stirring at 45° C. for 3 h, centrifuging (6000 rpm for 6 min), washing (washing with anhydrous ethanol 3 times), and drying (drying at 50° C. for 12 h) to obtain a pretreated intermediate product; (4) The pretreated intermediate product and the dispersant are ultrasonically dispersed in a mixture of ethanol and ethyl acetate in an amount of 10 times by weight, and then styrene monomer is added, emulsified for 25 minutes, and then the temperature is raised to 60° C., an initiator is added, and the mixture is reacted at 55° C. for 8 hours, and then washed (washed 3 times with anhydrous ethanol) and dried (dried at 40° C. for 8 hours) to obtain a product.

[0044] Embodiment 15 A composite anti-core burning agent, which is different from Example 13 in that step (3) and step (4) are specifically as follows: (3) ultrasonically dispersing the intermediate product in a mixed solution of ethanol and deionized water, adjusting the pH to 5, adding a silane coupling agent, stirring at 55° C. for 2 h, centrifuging (6000 rpm for 6 min), washing (washing with anhydrous ethanol 3 times), and drying (drying at 50° C. for 12 h) to obtain a pretreated intermediate product; (4) The pretreated intermediate product and the dispersant are ultrasonically dispersed in a mixture of ethanol and ethyl acetate in an amount of 10 times by weight, and then styrene monomer is added, emulsified for 35 minutes, and then the temperature is raised to 70°C, an initiator is added, and the mixture is reacted at 55-65°C for 8 hours, and then washed (washed 3 times with anhydrous ethanol) and dried (dried at 40°C for 8 hours) to obtain a product.

[0045] Example 16 A composite anti-core burning agent, which is different from Example 1 in that the pre-treated intermediate product is 0.6% of the mass of the styrene monomer.

[0046] Embodiment 17 A composite anti-core burning agent, which is different from Example 1 in that the pre-treated intermediate product is 0.8% of the mass of the styrene monomer.

[0047] Comparative Example Comparative Example 1 A composite anti-core burning agent, which is different from Example 1 in that it is obtained by heating ST-508T, ST-1912 and ST-506 in corresponding weight ratios to 60° C. and stirring at 200 rpm for 20 minutes.

[0048] Comparative Example 2 A composite anti-core burning agent, which is different from Example 1 in that it is obtained by heating ST-508T, ST-1912 and ST-506 in corresponding weight ratios to 60°C, stirring at 200rpm for 20min, and then mixing with porous silica in a weight ratio of 1:0.4, wherein the porous silica is purchased from 500nm mesoporous silica of Beijing Zhongke Keyou Technology Co., Ltd.

[0049] Application Examples Application Example 1 A polyurethane sponge is prepared by mixing the following raw materials by weight as a foaming system: 100 kg of polyether 5631D, 2 kg of silicone oil L580, 9 kg of water, 105 kg of isocyanate, and 0.25 kg of triethylenediamine as a catalyst; 0.4 wt % of a composite anti-burning agent is also used in the mixed system of the above raw materials; the source of the composite anti-burning agent is shown in Table 2.

[0050] Application Example 2-17 A polyurethane sponge, which is different from Application Example 1 in that the source of the composite anti-burning agent is as shown in Table 2 Table 2 Sources of composite anti-burning agent in application examples 1-17 Application Examples Source of composite anti-burning agent Application Example 1 Example 1 Application Example 2 Example 2 Application Example 3 Example 3 Application Example 4 Example 4 Application Example 5 Example 5 Application Example 6 Example 6 Application Example 7 Example 7 Application Example 8 Example 8 Application Example 9 Example 9 Application Example 10 Example 10 Application Example 11 Embodiment 11 Application Example 12 Example 12 Application Example 13 Embodiment 13 Application Example 14 Embodiment 14 Application Example 15 Embodiment 15 Application Example 16 Example 16 Application Example 17 Embodiment 17 Application Example 18 A polyurethane sponge, which is different from Application Example 1 in that the amount of the composite anti-core burning agent used is 0.6wt%.

[0051] Application Example 19 A polyurethane sponge, which is different from Application Example 1 in that the amount of the composite anti-core burning agent used is 0.8wt%.

[0052] Application comparison Application Comparative Example 1 A polyurethane sponge, which is different from Application Example 1 in that the composite anti-core burning agent is obtained in Comparative Example 1, and the amounts of ST-508T, ST-1912 and ST-506 used are the same.

[0053] Application Comparative Example 2 A polyurethane sponge, which is different from Application Example 1 in that the composite anti-core burning agent is obtained in Comparative Example 2, and the amounts of ST-508T, ST-1912 and ST-506 used are the same.

[0054] Performance test samples: The polyurethane sponge obtained in Application Example 1-19 was used as test sample 1-19, and the polyurethane sponge obtained in Application Comparative Example 1-2 was used as control sample 1-2.

[0055] Test method: (1) Anti-burning effect test: measure the burning area of ​​the polyurethane sponge, and test samples 1-19 and control samples 1-2 are measured three times each, and the average value is recorded in Table 3; (2) Detection of volatile organic matter content, refer to the standard test method of PB VWL709. Place the polyurethane sponge sample in a heated glass tube, then continuously purge it with high-purity gas into a -150°C freezing trap, then raise the temperature to 280°C at a rate of 12°C / s, send the volatile organic matter sample into a gas chromatography system for separation, and finally detect each component by mass spectrometry to achieve qualitative and quantitative characterization results. This method can be used to determine volatile organic matter TVOC and atomized component FOG respectively.

[0056] Table 3 Test results of test samples 1-19 and control samples 1-2 Combining test samples 1-3 and control sample 1 and Table 3, it can be seen that the composite anti-burning agent obtained by coating the antioxidant with porous silica is more suitable for coping with the long-term high temperature in the center of the product during the foaming process of polyurethane sponge, and the coordination effect of various antioxidant components is relatively excellent, thereby significantly improving the burning of the polyurethane sponge and the volatilization of organic matter. The burning area, TVOC and FOG values ​​obtained by testing are relatively low. Combining control sample 2 and Table 3, it can be seen that if only a simple physical mixture of multiple antioxidants and porous silica is used, although it can bring about the improvement of anti-burning and low organic volatilization, the improvement is limited in terms of the burning area, TVOC and FOG values, and is far less excellent than the composite anti-burning agent obtained by coating the antioxidant with porous silica.

[0057] Combining test sample 1 and test samples 4-6 with Table 3, it can be seen that when the weight ratio of the antioxidant to the porous silica is 1:(0.36-0.47), it can be ensured that the composite anti-burning agent obtained by coating the antioxidant with porous silica can exert an excellent and stable improvement effect on the burning and organic volatilization of the polyurethane sponge after application; among them, when the weight ratio of the antioxidant to the porous silica is 1:0.4, the application effect of the composite anti-burning agent is the best.

[0058] Combining test samples 1 and test samples 7-12 with Table 3, it can be seen that in the preparation of the composite anti-burning agent, the mass ratio of hexadecyltrimethylammonium bromide, triethanolamine and distilled water is controlled to be (5-7):1:(380-420), the concentration of ethyl orthosilicate after addition is 0.5-1 mol / L, and the concentration of ammonia water after addition is 0.9-1.5 mol / L, which can ensure that the final composite anti-burning agent can exert excellent and stable corresponding effects after application, and the measured burning area, TVOC and FOG values ​​are also relatively excellent and stable.

[0059] Combining test samples 1 and 13-15 with Table 3, it can be seen that by forming an inorganic-organic hybrid structure on the surface of the composite anti-core agent, the synergistic effect between the various combined antioxidants in the composite anti-core agent is more excellently exerted, and thus the core burning and organic volatilization of the polyurethane sponge can bring better improvement effects, and the measured core burning area, TVOC and FOG values ​​are also significantly reduced. Combining test samples 16-17 with Table 3, it can be seen that in the preparation of the composite anti-core agent, making the pre-treated intermediate product 0.6-0.8% of the mass of the styrene monomer can ensure that the obtained composite anti-core agent has an excellent and stable application effect.

[0060] Combining test samples 1 and 18-19 with Table 3, it can be seen that applying the composite anti-core burning agent to the preparation of polyurethane sponge and controlling the addition amount of the composite anti-core burning agent to 0.4-0.8wt% can bring excellent and stable application effects, and meet the application requirements in improving the core burning and organic volatilization of the polyurethane sponge.

[0061] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A composite anti-core burning agent, characterized in that: The antioxidant is obtained by coating porous silica, and the preparation steps are as follows: S1. Mix cetyltrimethylammonium bromide, triethanolamine and distilled water, and stir at 75-85° C. for 30-50 min to obtain a mixed solution; S2, adding an antioxidant to the mixed solution, mixing evenly, then adding ethyl orthosilicate and ammonia water, reacting for 18-24 hours, centrifuging, washing, and drying to obtain; The antioxidant is a mixture of at least any two of ST-1912, ST-5067, and ST-508T; The weight ratio of the antioxidant to the porous silica is 1:(0.36-0.47).

2. The composite anti-core burning agent according to claim 1, characterized in that: The weight ratio of the antioxidant to the porous silica is 1:0.

4.

3. The composite anti-core burning agent according to claim 1, characterized in that: The antioxidant is composed of the following components in parts by weight: composition: ST-508T 5-20 copies; ST-1912 50-65 copies; ST-5067 25-40 servings.

4. The composite anti-core burning agent according to claim 1, characterized in that: The mass ratio of hexadecyltrimethylammonium bromide, triethanolamine and distilled water is (5-7):1:(380-420).

5. The composite anti-core burning agent according to claim 1, characterized in that: In step S2, the concentration of ethyl orthosilicate after addition is 0.5-1 mol / L.

6. The composite anti-core burning agent according to claim 1, characterized in that: In step S2, the concentration of ammonia water after addition is 0.9-1.5 mol / L.

7. The composite anti-core burning agent according to claim 1, characterized in that: The antioxidant is obtained by coating the porous silica and then performing surface modification, and the preparation steps are as follows: (1) Mix cetyltrimethylammonium bromide, triethanolamine and distilled water, and stir at 75-85° C. for 30-50 minutes to obtain a mixed solution; (2) adding an antioxidant to the mixed solution, mixing well, then adding ethyl orthosilicate and ammonia water, reacting for 18-24 hours, and then centrifuging, washing, and drying to obtain an intermediate product; (3) ultrasonically dispersing the intermediate product in a mixed solution of ethanol and deionized water, adjusting the pH to 4-5, adding a silane coupling agent, stirring at 45-55° C. for 2-3 hours, centrifuging, washing, and drying to obtain a pretreated intermediate product; (4) Ultrasonic dispersion of the pretreated intermediate product and the dispersant in a mixture of ethanol and ethyl acetate, then adding styrene monomer, emulsifying for 25-35 minutes, then heating to 60-70°C, adding an initiator, reacting at 55-65°C for 6-8 hours, and washing and drying to obtain; The antioxidant is a mixture of at least any two of ST-1912, ST-5067, and ST-508T; The weight ratio of the antioxidant to the porous silica is 1:(0.36-0.47).

8. The composite anti-core burning agent according to claim 7, characterized in that: The pre-treated intermediate product accounts for 0.6-0.8% of the mass of the styrene monomer.

9. The use of a composite anti-core burning agent according to any one of claims 1 to 8, characterized in that: The composite anti-core burning agent is used in the preparation of polyurethane sponge, and the addition amount of the composite anti-core burning agent is 0.4-0.8wt%.

Citation Information

Patent Citations

  • Unsaturated polyester composite decorative board and manufacturing method thereof

    CN106280352A

  • Organic antioxidant-silica coated composite material as well as preparation method and application thereof

    CN107011969A

  • Preparation method of heat-resistant and wear-resistant modified polyurethane elastomer material

    CN108948725A

  • Impact-resistant MPP power cable protection tube and production process thereof

    CN112898684A

  • Thioester antioxidant production process and thioester antioxidant

    CN115232045A