Asphalt pavement sealant with high microwave absorptivity as well as preparation method and microwave heating in-situ repair method thereof
By designing asphalt pavement sealants with high microwave absorption rates and using microwave heating technology, the problem of limited self-healing ability of sealant materials is solved, efficient self-healing of the sealant and crack wall bonding are achieved, and the service life of the sealant is extended. service life and solves the problem of aging failure.
Patent Information
- Application Number
- CN202410885058.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-22
AI Technical Summary
Existing sealant materials have limited self-healing capabilities in asphalt pavement crack treatment, and are prone to failure due to aging and temperature changes, shortening the service life of the pavement.
Design an asphalt pavement sealant with high microwave absorption rate. Microwave heating technology is used to improve the self-healing efficiency of the sealant and the bonding performance with the crack wall. It uses 35 to 55 parts of base asphalt and 2 to 12 parts of SBS. sexual agent, The ratio of 15 to 40 parts of waste tire rubber powder, 8 to 19 parts of plasticizer, 0.05 to 2.75 parts of stabilizer and 4 to 20 parts of high microwave absorptivity filler is achieved through microwave heating in-situ repair method Quick fix.
Extend the service life of the sealant material, improve the self-healing performance of the sealant and the bonding performance with the crack wall, achieve rapid repair of aging and failed sealant, and effectively solve the problems of micro-cracks and debonding of the sealant material.
Smart Images

Figure CN118813201A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of asphalt pavement sealant repair. Background Art
[0002] Cracks are the most common disease of asphalt pavements, which seriously affect the long-term performance and service life of the pavement. Using hot-fill sealants to fill cracks in asphalt pavements is a common treatment method for cracking diseases. However, due to the complex road service environment and the repeated action of vehicle dynamic loads, pavement cracks are the weakest part of the pavement structure. The sealants are easily prone to self-cracking and debonding from the crack walls due to aging, and sealant failure occurs, resulting in the reappearance of cracks and further aggravation of the disease, shortening the service life of the asphalt pavement.
[0003] As a typical viscoelastic material, asphalt has the inherent property of self-healing, which can delay the generation and expansion of microcracks in asphalt pavement to a certain extent. Common hot-pouring sealants are mostly polymer-based composite materials based on asphalt, especially modified with SBS, TPS, rubber powder and stabilizers to show typical self-healing properties. Studies have shown that sealants will also produce periodic deformation under the action of the natural environment. The lower ambient temperature in winter causes microcracks on the surface of the sealant under the tensile action of temperature stress, accompanied by debonding from the crack wall; in the spring of the following year, the temperature rise reduces the temperature shrinkage stress, the width of the pavement cracks is smaller, and the sealant microcracks will also produce a certain degree of self-healing, which shows that the self-healing characteristics of the sealant material are significantly affected by temperature, but the temperature of the environment changes relatively slowly, and at the same time, it is affected by factors such as load and aging, and the self-healing ability of the sealant material is very limited. Summary of the invention
[0004] The present invention aims to solve the problem of limited self-healing ability of existing sealant materials, and further provides an asphalt pavement sealant with high microwave absorption rate, a preparation method thereof, and a microwave heating in-situ repair method.
[0005] A high microwave absorption rate asphalt pavement sealant is prepared from 35 to 55 parts of base asphalt, 2 to 12 parts of SBS modifier, 15 to 40 parts of waste tire rubber powder, 8 to 19 parts of plasticizer, 0.05 to 2.75 parts of stabilizer and 4 to 20 parts of high microwave absorption rate filler in parts by mass.
[0006] A method for preparing an asphalt pavement sealant with high microwave absorptivity is carried out according to the following steps:
[0007] 1. Weighing:
[0008] Weigh 35 to 55 parts of base asphalt, 2 to 12 parts of SBS modifier, 15 to 40 parts of waste tire rubber powder, 8 to 19 parts of plasticizer, 0.05 to 2.75 parts of stabilizer and 4 to 20 parts of high microwave absorption filler by mass;
[0009] 2. Shear and swelling of SBS modifier:
[0010] The weighed base asphalt is heated to a fluid state, and then the SBS modifier is added and heated and high-speed sheared to fully swell the SBS modifier, and then the stabilizer is added and heated and high-speed sheared to obtain an asphalt-based solution in which the SBS modifier is sheared and swollen;
[0011] 3. Pre-swelling of waste tire rubber powder:
[0012] The weighed waste tire rubber powder is mixed with a plasticizer, and then heated to swell to obtain pre-swelled waste tire rubber powder containing the plasticizer;
[0013] 4. Shearing of waste tire rubber powder:
[0014] The pre-swelled waste tire rubber powder containing a plasticizer is added to the asphalt-based solution sheared and swollen by the SBS modifier and heated and sheared at a high speed to obtain a mixed system;
[0015] 5. Mineral powder shearing with high microwave absorption rate:
[0016] Add the weighed filler with high microwave absorption rate to the mixed system, and then heat and shear at high speed until it is evenly dispersed to obtain a dispersed mixed system;
[0017] 6. Heating and stirring:
[0018] The dispersed mixed system is heated and stirred to complete the preparation method of the asphalt pavement sealant with high microwave absorption rate.
[0019] A microwave heating in-situ repair method for an asphalt pavement sealant with high microwave absorption rate is carried out according to the following steps:
[0020] 1. Clean the debris and dust on the surface of the aged and ineffective asphalt pavement sealant with high microwave absorption rate and around the cracks on the asphalt pavement;
[0021] 2. Under the conditions of electromagnetic wave frequency of 2GHz~4GHz and heating temperature of 80℃~150℃, the aged and failed asphalt pavement sealant with high microwave absorption rate is heated to a flowing state, and then compacted to make the flowing sealant fully fill the cracks, and finally cooled naturally, thus completing the microwave heating in-situ repair method of the asphalt pavement sealant with high microwave absorption rate.
[0022] The beneficial effects of the present invention are:
[0023] 1. The present invention makes full use of the self-healing properties and high-temperature flow properties of asphalt-based sealant materials, designs a sealant material with high microwave absorptivity, and uses microwave thermal induction technology to improve the self-healing efficiency of the sealant material and the adhesion performance with the crack wall, thereby extending the service life of the sealant material. The material is easy to obtain, the technology and process application conditions are mature, and it has strong popularization.
[0024] 2. The present invention can realize the in-situ rapid repair of aged and failed sealant materials through the above material preparation process, equipment design method and construction process, improve the self-healing performance of the sealant material, and quickly repair the microcracks of the aged and failed sealant material itself and the debonding between the aged and failed sealant material and the crack wall, thereby effectively extending the service life of the sealant material. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is an overall stereogram of the handheld in-situ repair device in the ninth embodiment;
[0026] Figure 2 It is a front schematic diagram of the handheld in-situ repair device in the ninth embodiment;
[0027] Figure 3 It is a top view schematic diagram of the handheld in-situ repair device in the ninth embodiment;
[0028] Figure 4 It is a front cross-sectional schematic diagram of the handheld in-situ repair device in the ninth embodiment;
[0029] Figure 5 It is a schematic diagram of working modules in the handheld in-situ repair device in the ninth embodiment;
[0030] Figure 6 This is a schematic diagram of a microwave emission module in a handheld in-situ repair device in a ninth embodiment;
[0031] Figure 7 It is a schematic diagram of a power module in the handheld in-situ repair device in the ninth embodiment. DETAILED DESCRIPTION
[0032] Specific implementation method 1: This implementation method is an asphalt pavement sealant with high microwave absorption rate, which is prepared by 35 to 55 parts of base asphalt, 2 to 12 parts of SBS modifier, 15 to 40 parts of waste tire rubber powder, 8 to 19 parts of plasticizer, 0.05 to 2.75 parts of stabilizer and 4 to 20 parts of high microwave absorption filler in parts by mass.
[0033] The beneficial effects of this specific implementation are:
[0034] 1. This specific implementation method makes full use of the self-healing properties and high-temperature flow properties of asphalt-based sealant materials. By designing a sealant material with high microwave absorptivity, the self-healing efficiency of the sealant material and the bonding performance with the crack wall are improved by microwave thermal induction technology, thereby extending the service life of the sealant material. The material is easy to obtain, the technology and process application conditions are mature, and it has strong popularization.
[0035] 2. This specific implementation method can achieve the in-situ rapid repair of aged and failed sealant materials through the above material preparation process, equipment design method and construction process, improve the self-healing performance of the sealant material, and quickly repair the microcracks of the aged and failed sealant material itself and the debonding between the aged and failed sealant material and the crack wall, thereby effectively extending the service life of the sealant material.
[0036] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that: the base asphalt is one of No. 70 base asphalt, No. 90 base asphalt and No. 110 base asphalt or a mixture of several of them; the SBS modifier is a star-shaped modifier or a mixture of a star-shaped modifier and a linear modifier, the ash content of the SBS modifier is not more than 0.2%, and the elongation at break is not less than 700%; the particle size of the waste tire rubber powder is 40 mesh to 100 mesh, and the density is 1.05g / cm 3 ~1.28g / cm 3 , the water content is not more than 1%; the plasticizer is one of furfural oil, epoxidized soybean oil, aromatic oil, castor oil, soybean oil, naphthenic oil and palm oil or a mixture of several of them; the stabilizer is sulfur powder, the apparent density is 0.6g / cm 3 ~0.8g / cm 3 The high microwave absorption filler is one of steel slag powder, tourmaline powder, basalt powder, diabase powder, andesite powder, hydroxy iron powder, carbon black powder, silicon carbide and graphene, or a mixture of several of them; the particle size of the high microwave absorption filler is ≤200 mesh. The rest is the same as the first embodiment.
[0037] Specific implementation method three: This implementation method is a method for preparing an asphalt pavement sealant with high microwave absorption rate, which is carried out according to the following steps:
[0038] 1. Weighing:
[0039] Weigh 35 to 55 parts of base asphalt, 2 to 12 parts of SBS modifier, 15 to 40 parts of waste tire rubber powder, 8 to 19 parts of plasticizer, 0.05 to 2.75 parts of stabilizer and 4 to 20 parts of high microwave absorption filler by mass;
[0040] 2. Shear and swelling of SBS modifier:
[0041] The weighed base asphalt is heated to a fluid state, and then the SBS modifier is added and heated and high-speed sheared to fully swell the SBS modifier, and then the stabilizer is added and heated and high-speed sheared to obtain an asphalt-based solution in which the SBS modifier is sheared and swollen;
[0042] 3. Pre-swelling of waste tire rubber powder:
[0043] The weighed waste tire rubber powder is mixed with a plasticizer, and then heated to swell to obtain pre-swelled waste tire rubber powder containing the plasticizer;
[0044] 4. Shearing of waste tire rubber powder:
[0045] The pre-swelled waste tire rubber powder containing a plasticizer is added to the asphalt-based solution sheared and swollen by the SBS modifier and heated and sheared at a high speed to obtain a mixed system;
[0046] 5. Mineral powder shearing with high microwave absorption rate:
[0047] Add the weighed filler with high microwave absorption rate to the mixed system, and then heat and shear at high speed until it is evenly dispersed to obtain a dispersed mixed system;
[0048] 6. Heating and stirring:
[0049] The dispersed mixed system is heated and stirred to complete the preparation method of the asphalt pavement sealant with high microwave absorption rate.
[0050] In step 2 of this specific implementation method, SBS forms a cross-linked structure in asphalt.
[0051] In step 3 of this specific implementation method, it is ensured that the waste tire rubber powder has sufficient light components for pre-swelling
[0052] In step six of this specific implementation method, each polymer modifier is promoted to be fully cross-linked in the asphalt to form an interpenetrating network structure, and the high microwave absorption rate mineral powder is sheared and dispersed uniformly.
[0053] Specific embodiment 4: This embodiment is different from specific embodiment 3 in that: in step 2, the weighed base asphalt is heated to 110°C to 180°C to reach a fluid state, then the SBS modifier is added, and the mixture is stirred for 5min to 120min at a temperature of 110°C to 180°C and a rotation speed of 200rpm to 3000rpm, and then the mixture is heated to 150°C to 215°C after stirring, and heated at a high speed shear for 10min to 90min at a temperature of 150°C to 215°C and a rotation speed of 1000rpm to 10000rpm to fully swell the SBS modifier, and then the stabilizer is added, and the mixture is heated at a high speed shear for 5min to 60min at a temperature of 150°C to 215°C and a rotation speed of 1000rpm to 10000rpm to obtain an asphalt-based solution sheared and swollen by the SBS modifier. The rest is the same as specific embodiment 3.
[0054] Specific embodiment 5: This embodiment is different from specific embodiment 3 or 4 in that: in step 3, the weighed waste tire rubber powder is mixed with a plasticizer, and then heated and swelled for 10 minutes to 120 minutes at a temperature of 110° C. to 180° C. to obtain pre-swelled waste tire rubber powder containing a plasticizer. The rest is the same as specific embodiment 3 or 4.
[0055] Specific embodiment 6: This embodiment is different from the specific embodiments 3 to 5 in that: in step 4, under the condition of a temperature of 110°C to 180°C, the pre-swelled waste tire rubber powder containing a plasticizer is added to the asphalt-based solution sheared and swollen by the SBS modifier, and then the temperature is raised to 150°C to 225°C, and the high-speed shearing is performed for 10min to 120min at a temperature of 150°C to 225°C and at 1000rpm to 10000rpm to obtain a mixed system. The rest is the same as the specific embodiments 3 to 5.
[0056] Specific embodiment 7: This embodiment is different from any one of specific embodiments 3 to 6 in that: in step 5, under the condition of a temperature of 150°C to 225°C, a weighed high microwave absorption filler is added to the mixed system, and then heated and high-speed sheared for 5min to 60min under the condition of a temperature of 150°C to 225°C and a rotation speed of 1000rpm to 10000rpm to obtain a dispersed mixed system; in step 6, under the condition of a temperature of 150°C to 180°C and a rotation speed of 100rpm to 1000rpm, the dispersed mixed system is heated and stirred for 5min to 200min. The rest is the same as specific embodiments 3 to 6.
[0057] Specific embodiment eight: This embodiment is a microwave heating in-situ repair method of an asphalt pavement sealant with high microwave absorption rate, which is carried out according to the following steps:
[0058] 1. Clean the debris and dust on the surface of the aged and ineffective asphalt pavement sealant with high microwave absorption rate and around the cracks on the asphalt pavement;
[0059] 2. Under the conditions of electromagnetic wave frequency of 2GHz~4GHz and heating temperature of 80℃~150℃, the aged and failed asphalt pavement sealant with high microwave absorption rate is heated to a flowing state, and then compacted to make the flowing sealant fully fill the cracks, and finally cooled naturally, thus completing the microwave heating in-situ repair method of the asphalt pavement sealant with high microwave absorption rate.
[0060] Step 1 of this specific implementation method is to clean up the debris and dust around the aged and failed sealant to ensure that the surface of the aged and failed sealant material is clean and tidy, improve the heating efficiency and repair effect of the aged and failed sealant material, and use a blower to blow the surface of the aged and failed sealant and the surrounding areas of its cracks during cleaning.
[0061] In step 2 of this specific implementation method, a handheld in-situ repair device can be used to in-situ repair the heated aged and failed sealant on the asphalt pavement until it is in a fully flowing state, so as to ensure that the cracks in the sealant material are fully self-healed and re-bonded to the crack wall.
[0062] Step 2 of this specific implementation method utilizes a tamping hammer for tamping. After the aged and failed sealant is fully heated, further external force is used to allow the sealant material to fully fill the cracks, thereby improving the self-healing degree of the aged and failed sealant material and the degree of adhesion to the crack wall. The tamping hammer should be a rubber hammer, and Vaseline should be applied to the rubber hammer before tamping to avoid the sealant material from sticking to the tamping hammer.
[0063] Specific implementation method nine, combined with Figures 1 to 7 Specific description: The difference between this embodiment and the eighth embodiment is that: in step 2, the aged and failed asphalt pavement sealant with high microwave absorption rate is heated to a flowing state by using a handheld in-situ repair device; the handheld in-situ repair device is composed of a display module 1, a handle 2, a housing 3, a working module 4, a monitoring unit 5, a microwave transmitting module 7 and a power module 8;
[0064] The housing 3 is formed by connecting a straight tube structure and a tube structure with a bent end, and the diameter of the straight tube structure is larger than the tube structure with a bent end; a handle 2 is arranged at the lower part of the straight tube structure, and a display module 1 is arranged at the end of the straight tube structure;
[0065] A monitoring unit 5, a microwave transmitting module 7 and a power supply module 8 are arranged inside the straight tube structure; the microwave transmitting module 7 is composed of a magnetron 11 and an antenna 12;
[0066] A working module 4 is arranged inside the tube structure with a bent end, and the working module 4 is composed of a waveguide 6 and a temperature sensor 9. The temperature sensor 9 is arranged inside the bent end and is used to monitor the temperature of the sealant at the heated position in real time. The waveguide 6 is arranged along the length direction of the tube structure with a bent end. One end of the waveguide 6 is connected to an antenna 12, and the antenna 12 is arranged on a magnetron 11.
[0067] The monitoring unit 5 is used to monitor the temperature sensor 9 in real time and control the working power of the magnetron 11; the display module 1 is connected to the monitoring unit 5 and the power module 8 for displaying information and control; the power module 8 is respectively connected to the display module 1, the working module 4, the monitoring unit 5 and the microwave transmitting module 7. The rest is the same as the specific embodiment eight.
[0068] In this specific embodiment, the handle 2 is used to facilitate the device user to hold the device. The shell 3 is made of high-temperature resistant material and has a streamlined appearance to facilitate the operator to hold the device. The display module 1 is used to display device information such as the sealant temperature at the heated position and the working power of the microwave emission module 7. The working module 4 is used for direct contact between the device and the road surface, and the waveguide 6 in the working module 4 is used to transmit the microwave energy output by the antenna 12.
[0069] The temperature sensor 9 of this specific embodiment is an infrared temperature sensor, which is used to monitor the temperature of the sealant at the heated position in real time, and is convenient for accurately monitoring the temperature of the sealant at the heated position without contact; the monitoring unit 5 controls the working power of the magnetron 11 according to the temperature of the sealant at the heated position, and increases the working power of the magnetron 11 when the temperature of the sealant at the heated position is lower than the preset temperature, and reduces the working power of the magnetron 11 when the temperature of the sealant at the heated position is higher than the preset temperature;
[0070] In this specific embodiment, the magnetron 11 is used to generate and transmit microwave signals and adjust the working power according to the output signal of the monitoring unit 5 . The antenna 12 is used to transmit and amplify the microwaves generated by the magnetron 11 .
[0071] Specific embodiment 10: This embodiment is different from specific embodiment 8 or 9 in that: the material of the housing 3 is high temperature resistant material; the power module 8 includes a storage battery 13 and a transformer 14; the magnetron 11 is connected to the storage battery 13 through the transformer 14; the curved end of the curved end of the cylindrical structure is provided with a roller 10, and the roller 10 is a universal wheel. The rest is the same as specific embodiment 8 or 9.
[0072] The present embodiment uses rollers 10 to partially isolate the working module 4 from the road surface, making it easier for the operator to move the device. The power module 8 provides power for the entire device, and the transformer 14 is used to convert the on-site power supply voltage into the working voltage required by the magnetron 11.
[0073] The following examples are used to verify the beneficial effects of the present invention:
[0074] Embodiment 1:
[0075] The invention discloses an asphalt pavement sealant with high microwave absorption rate, which is prepared from 40 parts of base asphalt, 6 parts of SBS modifier, 25 parts of waste tire rubber powder, 10 parts of plasticizer, 0.5 parts of stabilizer and 15 parts of filler with high microwave absorption rate in parts by mass.
[0076] The base asphalt is No. 70 base asphalt; the SBS modifier is the YH-791 SBS modifier purchased by Yucheng (Hongji) Plastic Dongguan Co., Ltd.; the waste tire rubber powder is a waste tire rubber powder with a particle size of 40 to 100 meshes obtained by hot-mechanical extrusion and shearing process, and a density of 1.13 g / cm 3 , the water content is 0.41%; the plasticizer is aromatic oil, the effective component mass percentage is not less than 95%; the stabilizer is sulfur powder, the apparent density is 0.7g / cm 3 The high microwave absorption filler is a mixture of steel slag powder, tourmaline powder and graphene in a mass ratio of 2:1:2; the particle size of the high microwave absorption filler is 200 mesh. The aromatic oil is TC-24 aromatic oil purchased from Shandong Taichang Petrochemical Technology Co., Ltd.
[0077] The method for preparing the asphalt pavement sealant with high microwave absorptivity is carried out according to the following steps:
[0078] 1. Weighing:
[0079] Weigh 40 parts of base asphalt, 6 parts of SBS modifier, 25 parts of waste tire rubber powder, 10 parts of plasticizer, 0.5 parts of stabilizer and 15 parts of high microwave absorption filler by mass;
[0080] 2. Shear and swelling of SBS modifier:
[0081] The weighed base asphalt is heated to 150°C to reach a fluid state, and then the SBS modifier is added, and stirred for 60 minutes at a temperature of 150°C and a rotation speed of 1500rpm. After stirring, the temperature is raised to 200°C, and heated at a high speed shear for 50 minutes at a temperature of 200°C and a rotation speed of 7000rpm to fully swell the SBS modifier, and then the stabilizer is added, and the temperature is kept at 200°C and a rotation speed of 7000rpm. The high-speed shear is continued for 30 minutes to obtain an asphalt-based solution in which the SBS modifier is sheared and swollen;
[0082] 3. Pre-swelling of waste tire rubber powder:
[0083] The weighed waste tire rubber powder is mixed with a plasticizer, and then heated and swelled at 150° C. for 60 minutes to obtain pre-swelled waste tire rubber powder containing a plasticizer;
[0084] 4. Shearing of waste tire rubber powder:
[0085] At a temperature of 150°C, the pre-swollen waste tire rubber powder containing a plasticizer was added to the asphalt-based solution sheared and swollen by the SBS modifier, and then the temperature was raised to 210°C, and the mixture was heated and high-speed sheared for 60 minutes at a temperature of 210°C and a speed of 8000 rpm to obtain a mixed system;
[0086] 5. Mineral powder shearing with high microwave absorption rate:
[0087] Under the condition of temperature of 180° C., the weighed filler with high microwave absorption rate is added to the mixed system, and then heated and high-speed sheared for 30 minutes under the condition of temperature of 180° C. and rotation speed of 6000 rpm to obtain a dispersed mixed system;
[0088] 6. Heating and stirring:
[0089] Under the conditions of a temperature of 150° C. and a rotation speed of 500 rpm, the dispersed mixed system is heated and stirred for 60 minutes, thereby completing the preparation method of the asphalt pavement sealant with high microwave absorption rate.
[0090] Embodiment 2:
[0091] A high microwave absorption rate asphalt pavement sealant is prepared from 50 parts of base asphalt, 4 parts of SBS modifier, 30 parts of waste tire rubber powder, 15 parts of plasticizer, 1 part of stabilizer and 10 parts of high microwave absorption rate filler by mass.
[0092] The base asphalt is No. 90 base asphalt; the SBS modifier is the YH-791 SBS modifier purchased by Yucheng (Hongji) Plastic Dongguan Co., Ltd.; the waste tire rubber powder is a waste tire rubber powder with a particle size of 40 to 100 meshes obtained by thermal-mechanical extrusion and shearing process, and a density of 1.13 g / cm 3 , the water content is 0.41%; the plasticizer is a mixture of epoxidized soybean oil and aromatic oil in a mass ratio of 2:1, and the mass percentage of the effective ingredient is not less than 98%; the stabilizer is sulfur powder, and the apparent density is 0.7g / cm 3The high microwave absorption filler is a mixture of diabase powder, hydroxy iron powder and carbon black powder in a mass ratio of 2:1:1; the particle size of the high microwave absorption filler is 200 mesh. The epoxidized soybean oil is an epoxidized soybean oil with an epoxide value of 6.3 purchased from Jinan Luying Chemical Co., Ltd.; the aromatic oil is TC-24 aromatic oil purchased from Shandong Taichang Petrochemical Technology Co., Ltd.
[0093] The method for preparing the asphalt pavement sealant with high microwave absorptivity is carried out according to the following steps:
[0094] 1. Weighing:
[0095] Weigh 50 parts of base asphalt, 4 parts of SBS modifier, 30 parts of waste tire rubber powder, 15 parts of plasticizer, 1 part of stabilizer and 10 parts of high microwave absorption filler by mass;
[0096] 2. Shear and swelling of SBS modifier:
[0097] The weighed base asphalt is heated to 130°C to reach a fluid state, and then the SBS modifier is added, and stirred for 45 minutes at a temperature of 130°C and a rotation speed of 2500rpm, and then the temperature is raised to 190°C after stirring, and heated at a high speed shear for 40 minutes at a temperature of 190°C and a rotation speed of 9000rpm to fully swell the SBS modifier, and then the stabilizer is added, and the temperature is kept at 190°C and a rotation speed of 9000rpm. The high-speed shear is continued for 45 minutes to obtain an asphalt-based solution in which the SBS modifier is sheared and swollen;
[0098] 3. Pre-swelling of waste tire rubber powder:
[0099] The weighed waste tire rubber powder is mixed with a plasticizer, and then heated and swelled for 45 minutes at a temperature of 130° C. to obtain pre-swelled waste tire rubber powder containing a plasticizer;
[0100] 4. Shearing of waste tire rubber powder:
[0101] At a temperature of 150°C, the pre-swollen waste tire rubber powder containing plasticizer is added to the asphalt-based solution sheared and swollen by the SBS modifier, and then the temperature is raised to 200°C, and the mixture is heated and high-speed sheared for 45 minutes at a temperature of 200°C and at 9000 rpm to obtain a mixed system;
[0102] 5. Mineral powder shearing with high microwave absorption rate:
[0103] Under the condition of temperature of 160° C., the weighed filler with high microwave absorption rate is added to the mixed system, and then the system is heated and high-speed sheared for 40 minutes under the condition of temperature of 160° C. and rotation speed of 8000 rpm to obtain a dispersed mixed system;
[0104] 6. Heating and stirring:
[0105] Under the conditions of a temperature of 150° C. and a rotation speed of 800 rpm, the dispersed mixed system is heated and stirred for 90 minutes, thereby completing the preparation method of the asphalt pavement sealant with high microwave absorption rate.
[0106] Embodiment three:
[0107] The invention discloses an asphalt pavement sealant with high microwave absorption rate, which is prepared from 50 parts of base asphalt, 5 parts of SBS modifier, 25 parts of waste tire rubber powder, 10 parts of plasticizer, 0.8 parts of stabilizer and 20 parts of filler with high microwave absorption rate by mass.
[0108] The base asphalt is No. 70 base asphalt; the SBS modifier is the YH-791 SBS modifier purchased by Yucheng (Hongji) Plastic Dongguan Co., Ltd.; the waste tire rubber powder is a waste tire rubber powder with a particle size of 40 to 100 meshes obtained by hot-mechanical extrusion and shearing process, and a density of 1.13 g / cm 3 , the water content is 0.41%; the plasticizer is a mixture of naphthenic oil and aromatic oil in a mass ratio of 1:2, and the mass percentage of the effective component is not less than 98%; the stabilizer is sulfur powder, with an apparent density of 0.75g / cm 3 The high microwave absorption filler is a mixture of steel slag powder, basalt powder and graphene in a mass ratio of 1:2:1; the particle size of the high microwave absorption filler is 200 mesh. The naphthenic oil is KN4006 naphthenic oil purchased by Jinan Luying Chemical Co., Ltd.; the aromatic oil is TC-24 aromatic oil purchased by Shandong Taichang Petrochemical Technology Co., Ltd.
[0109] The method for preparing the asphalt pavement sealant with high microwave absorptivity is carried out according to the following steps:
[0110] 1. Weighing:
[0111] Weigh 50 parts of base asphalt, 5 parts of SBS modifier, 25 parts of waste tire rubber powder, 10 parts of plasticizer, 0.8 parts of stabilizer and 20 parts of high microwave absorption filler by mass;
[0112] 2. Shear and swelling of SBS modifier:
[0113] The weighed base asphalt is heated to 140°C to reach a fluid state, and then the SBS modifier is added, and stirred for 50 minutes at a temperature of 140°C and a rotation speed of 3000 rpm, and then the temperature is raised to 195°C after stirring, and heated and high-speed sheared for 35 minutes at a temperature of 195°C and a rotation speed of 10000 rpm to fully swell the SBS modifier, and then the stabilizer is added, and the temperature is kept at 195°C and a rotation speed of 10000 rpm. Shearing for 35 minutes to obtain an asphalt-based solution in which the SBS modifier is sheared and swollen;
[0114] 3. Pre-swelling of waste tire rubber powder:
[0115] The weighed waste tire rubber powder is mixed with a plasticizer, and then heated and swelled for 50 minutes at a temperature of 140° C. to obtain pre-swelled waste tire rubber powder containing a plasticizer;
[0116] 4. Shearing of waste tire rubber powder:
[0117] At a temperature of 180°C, the pre-swollen waste tire rubber powder containing a plasticizer was added to the asphalt-based solution sheared and swollen by the SBS modifier, and then the temperature was raised to 205°C, and the mixture was heated and high-speed sheared for 50 minutes at a temperature of 205°C and a speed of 10,000 rpm to obtain a mixed system;
[0118] 5. Mineral powder shearing with high microwave absorption rate:
[0119] Under the condition of temperature of 180° C., the weighed filler with high microwave absorption rate is added to the mixed system, and then the system is heated and high-speed sheared for 45 minutes under the condition of temperature of 180° C. and rotation speed of 9000 rpm to obtain a dispersed mixed system;
[0120] 6. Heating and stirring:
[0121] Under the conditions of a temperature of 160° C. and a rotation speed of 600 rpm, the dispersed mixed system is heated and stirred for 75 minutes, thereby completing the preparation method of the asphalt pavement sealant with high microwave absorption rate.
[0122] The performance of the asphalt pavement sealant with high microwave absorption rate prepared in Examples 1 to 3 was tested, as shown in Table 1:
[0123] Table 1
[0124]
[0125]
[0126] By testing various evaluation indicators of the asphalt pavement sealants prepared in Example 1, Example 2 and Example 3, it can be seen that the sealants of all examples can meet the basic requirements of viscosity, elastic recovery rate, ductility, low temperature flexibility, high temperature stability, adhesion, etc., showing good construction performance and durability. At the same time, in terms of anti-aging performance, water resistance and other aspects, each example also performs well and can meet the needs of actual engineering applications.
[0127] It is worth noting that in terms of microwave absorption rate, the sealant prepared in Example 1 shows the most excellent performance, and its RL value is the lowest, indicating that the sealant has the strongest microwave absorption capacity. This is mainly due to the optimization of raw material selection and preparation process in Example 1, by selecting a variety of mineral powders with high microwave absorption rates for mixed use, and adopting high-speed shearing and full cross-linking methods in the preparation process, so that the mineral powder is evenly dispersed in the asphalt, thereby improving the microwave absorption capacity of the sealant.
[0128] Embodiment 4: The microwave heating in-situ repair method of the asphalt pavement sealant with high microwave absorption rate in Embodiment 1 is carried out according to the following steps:
[0129] 1. Clean the debris and dust on the surface of the aged and ineffective asphalt pavement sealant with high microwave absorption rate and around the cracks on the asphalt pavement;
[0130] 2. Under the conditions of an electromagnetic wave frequency of 2.45 GHz and a heating temperature of 100°C, a handheld in-situ repair device is used to heat the aged and failed asphalt pavement sealant with high microwave absorption rate to a flowing state, and then the flowing sealant is compacted to fully fill the cracks, and finally cooled naturally, thereby completing the microwave heating in-situ repair method of the asphalt pavement sealant with high microwave absorption rate.
[0131] The handheld in-situ repair device is composed of a display module 1, a handle 2, a housing 3, a working module 4, a monitoring unit 5, a microwave transmitting module 7 and a power supply module 8;
[0132] The housing 3 is formed by connecting a straight tube structure and a tube structure with a bent end, and the diameter of the straight tube structure is larger than the tube structure with a bent end; a handle 2 is arranged at the lower part of the straight tube structure, and a display module 1 is arranged at the end of the straight tube structure;
[0133] A monitoring unit 5, a microwave transmitting module 7 and a power supply module 8 are arranged inside the straight tube structure; the microwave transmitting module 7 is composed of a magnetron 11 and an antenna 12;
[0134] A working module 4 is arranged inside the tube structure with a bent end, and the working module 4 is composed of a waveguide 6 and a temperature sensor 9. The temperature sensor 9 is arranged inside the bent end and is used to monitor the temperature of the sealant at the heated position in real time. The waveguide 6 is arranged along the length direction of the tube structure with a bent end. One end of the waveguide 6 is connected to an antenna 12, and the antenna 12 is arranged on a magnetron 11.
[0135] The monitoring unit 5 is used to monitor the temperature sensor 9 in real time and control the working power of the magnetron 11; the display module 1 is connected to the monitoring unit 5 and the power module 8 for displaying information and control; the power module 8 is respectively connected to the display module 1, the working module 4, the monitoring unit 5 and the microwave transmission module 7.
[0136] The shell 3 is made of high temperature resistant material; the power module 8 includes a storage battery 13 and a transformer 14; the magnetron 11 is connected to the storage battery 13 through the transformer 14; the bent end of the cylindrical structure with bent ends is provided with a roller 10, and the roller 10 is a universal wheel.
[0137] When using this specific embodiment, the user holds the handle 2, then turns on the power of the device through the display module 1 and sets the expected heating temperature, which is 100°C in this embodiment, and then uses the universal wheel of the roller 10 to align the end of the waveguide 6 under the working module 4 of the device with the heated object, which is the sealant material in the crack in this embodiment, and then moves the entire device along the crack to ensure that the sealant material in the crack is heated evenly, and when the sealant material with high microwave absorption rate is heated to the preset 100°C and reaches a flowing state, the next step is performed.
Claims
1. An asphalt pavement sealant with high microwave absorptivity, characterized in that It is prepared from 35 to 55 parts of base asphalt, 2 to 12 parts of SBS modifier, 15 to 40 parts of waste tire rubber powder, 8 to 19 parts of plasticizer, 0.05 to 2.75 parts of stabilizer and 4 to 20 parts of high microwave absorption filler in parts by mass.
2. The asphalt pavement sealant with high microwave absorptivity according to claim 1, characterized in that The base asphalt is one of No. 70 base asphalt, No. 90 base asphalt and No. 110 base asphalt, or a mixture of several thereof; the SBS modifier is a star-shaped modifier or a mixture of a star-shaped modifier and a linear modifier; the ash content of the SBS modifier is not more than 0.2%, and the elongation at break is not less than 700%; the particle size of the waste tire rubber powder is 40 mesh to 100 mesh, and the density is 1.05 g / cm 3 ~1.28g / cm 3 , the moisture content is not more than 1%; the plasticizer is one of furfural oil, epoxidized soybean oil, aromatic oil, castor oil, soybean oil, naphthenic oil and palm oil or a mixture of several of them; the stabilizer is sulfur powder with an apparent density of 0.6g / cm 3 ~0.8g / cm 3 ; The high microwave absorption filler is one or a mixture of steel slag powder, tourmaline powder, basalt powder, diabase powder, andesite powder, hydroxy iron powder, carbon black powder, silicon carbide and graphene; the particle size of the high microwave absorption filler is ≤200 mesh.
3. The method for preparing an asphalt pavement sealant with high microwave absorptivity according to claim 1, characterized in that It is carried out in the following steps:
1. Weigh: Weigh 35 to 55 parts of base asphalt, 2 to 12 parts of SBS modifier, 15 to 40 parts of waste tire rubber powder, 8 to 19 parts of plasticizer, 0.05 to 2.75 parts of stabilizer and 4 to 20 parts of high microwave absorption filler according to mass; 2. Shear and swelling of SBS modifier: The weighed base asphalt is heated to a fluid state, and then the SBS modifier is added and heated and sheared at high speed to fully swell the SBS modifier. Then, a stabilizer is added and heated and sheared at high speed to obtain an asphalt-based solution in which the SBS modifier is sheared and swollen.
3. Pre-swelling of waste tire rubber powder: The weighed waste tire rubber powder is mixed with a plasticizer, and then heated to swell to obtain pre-swollen waste tire rubber powder containing the plasticizer; 4. Shearing of waste tire rubber powder: The pre-swelled waste tire rubber powder containing plasticizer is added to the asphalt-based solution sheared and swollen by the SBS modifier and subjected to heating and high-speed shearing to obtain a mixed system; 5. Mineral powder shearing with high microwave absorption rate: Adding the weighed high microwave absorptivity filler to the mixed system, and then heating and high-speed shearing until the system is uniformly dispersed to obtain a dispersed mixed system; 6. Heating and stirring: The dispersed mixed system is heated and stirred to complete the preparation method of the asphalt pavement sealant with high microwave absorption rate.
4. The method for preparing an asphalt pavement sealant with high microwave absorptivity according to claim 3, characterized in that In step 2, the weighed base asphalt is heated to 110°C to 180°C to reach a fluid state, and then the SBS modifier is added. The mixture is stirred for 5min to 120min at a temperature of 110°C to 180°C and a rotation speed of 200rpm to 3000rpm. After stirring, the mixture is heated to 150°C to 215°C, and heated and sheared at a high speed for 10min to 90min at a temperature of 150°C to 215°C and a rotation speed of 1000rpm to 10000rpm to fully swell the SBS modifier. Then, the stabilizer is added, and the mixture is heated and sheared at a high speed for 5min to 60min at a temperature of 150°C to 215°C and a rotation speed of 1000rpm to 10000rpm to obtain an asphalt-based solution in which the SBS modifier is sheared and swollen.
5. The method for preparing an asphalt pavement sealant with high microwave absorptivity according to claim 3, characterized in that In step three, the weighed waste tire rubber powder is mixed with a plasticizer, and then heated and swelled at a temperature of 110° C. to 180° C. for 10 to 120 minutes to obtain pre-swelled waste tire rubber powder containing a plasticizer.
6. The method for preparing an asphalt pavement sealant with high microwave absorptivity according to claim 3, characterized in that In step 4, the pre-swelled waste tire rubber powder containing the plasticizer is added to the asphalt-based solution sheared and swollen by the SBS modifier at a temperature of 110° C. to 180° C., and then the temperature is raised to 150° C. to 225° C., and the mixture is heated at a high speed shearing speed of 10 min to 120 min at a temperature of 150° C. to 225° C. and at a speed of 1000 rpm to 10,000 rpm to obtain a mixed system.
7. The method for preparing an asphalt pavement sealant with high microwave absorptivity according to claim 3, characterized in that In step 5, the weighed high microwave absorptivity filler is added to the mixed system at a temperature of 150°C to 225°C, and then heated and high-speed sheared for 5min to 60min at a temperature of 150°C to 225°C and a rotation speed of 1000rpm to 10000rpm to obtain a dispersed mixed system; in step 6, the dispersed mixed system is heated and stirred for 5min to 200min at a temperature of 150°C to 180°C and a rotation speed of 100rpm to 1000rpm.
8. The microwave heating in-situ repair method of asphalt pavement sealant with high microwave absorptivity according to claim 1, characterized in that It is carried out in the following steps:
1. Clean the debris and dust on the surface of the asphalt pavement sealant with high microwave absorption rate and cracks on the asphalt pavement; 2. Under the conditions of electromagnetic wave frequency of 2GHz to 4GHz and heating temperature of 80℃ to 150℃, the aged and failed asphalt pavement sealant with high microwave absorption rate is heated to a flowing state, and then compacted to make the flowing sealant fully fill the cracks, and finally cooled naturally, thus completing the microwave heating in-situ repair method of the asphalt pavement sealant with high microwave absorption rate.
9. The microwave heating in-situ repair method of asphalt pavement sealant with high microwave absorptivity according to claim 8, characterized in that In step 2, a handheld in-situ repair device is used to heat the aged and failed asphalt pavement sealant with high microwave absorption rate to a flowing state; the handheld in-situ repair device is composed of a display module (1), a handle (2), a housing (3), a working module (4), a monitoring unit (5), a microwave emission module (7) and a power supply module (8); The housing (3) is formed by connecting a straight tube structure and a tube structure with a bent end, and the diameter of the straight tube structure is larger than that of the tube structure with a bent end; a handle (2) is provided at the lower part of the straight tube structure, and a display module (1) is provided at the end of the straight tube structure; A monitoring unit (5), a microwave transmitting module (7) and a power supply module (8) are arranged inside the straight cylindrical structure; the microwave transmitting module (7) is composed of a magnetron (11) and an antenna (12); A working module (4) is arranged inside the cylindrical structure with a bent end. The working module (4) is composed of a waveguide tube (6) and a temperature sensor (9). The temperature sensor (9) is arranged inside the bent end and is used to monitor the temperature of the sealant at the heated position in real time. The waveguide tube (6) is arranged along the length direction of the cylindrical structure with a bent end. One end of the waveguide tube (6) is connected to an antenna (12), and the antenna (12) is arranged on the magnetron (11). The monitoring unit (5) is used to monitor the temperature sensor (9) in real time and control the working power of the magnetron (11); the display module (1) is connected to the monitoring unit (5) and the power module (8) for displaying information and controlling; the power module (8) is respectively connected to the display module (1), the working module (4), the monitoring unit (5) and the microwave transmitting module (7).
10. The microwave heating in-situ repair method of asphalt pavement sealant with high microwave absorptivity according to claim 9, characterized in that The shell (3) is made of a high-temperature resistant material; the power module (8) includes a storage battery (13) and a transformer (14); the magnetron (11) is connected to the storage battery (13) via the transformer (14); and a roller (10) is provided at the curved end of the cylindrical structure with a curved end, and the roller (10) is a universal wheel.
Citation Information
Patent Citations
Environment-friendly low-grade hard asphalt modification method
CN111234547A
Application of asphalt pouring sealant in microwave heating maintenance of asphalt pavement
CN116377785A
Microwave heating in-situ intelligent self-repairing system for asphalt pavement cracks
CN117488639A
Non-cured rubber asphalt waterproof coating heating device
CN213755026U
Radio-absorbing asphalt-concrete road repair composition, method for manufacture and pouring thereof
RU2665541C1
Cited By
Pretreated crumb rubber-modified asphalt, and preparation method thereof, and use in emergency pavement repair
GB2701265A