Method for detecting longitudinal forming line defects of annealed steel plate for stamping

By uniaxially stretching the cold-rolled annealed sheet and then polishing it along the length direction, the longitudinal forming stripe defects are detected, which solves the problems of difficulty in detection and defect outflow in the existing technology, and improves product stability and market competitiveness.

CN118817455APending Publication Date: 2024-10-22BEIJING SHOUGANG CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410526692.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-29
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

It is difficult to detect longitudinal forming stripe defects in cold-rolled annealed plates in steel mill products with existing technology. As a result, these defects are discovered only after stamping, which affects the production rhythm and product credibility. It is also difficult to detect and easily leaked to users. .

Method used

By uniaxially stretching the cold-rolled annealed plate and then polishing it along the length direction, using a whetstone or gauze for inspection, multiple comparison samples are set to increase the stretching ratio to determine whether there are stripe defects on the polished surface and determine whether it is qualified or qualified. Unqualified.

Benefits of technology

It can effectively detect longitudinal forming stripe defects, prevent them from flowing out, improve the stability and market competitiveness of steel enterprises' products, and reduce economic losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118817455A_ABST
    Figure CN118817455A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of plate steel product defect inspection, in particular to a method for detecting longitudinal forming line defects of an annealed steel plate for stamping. The invention provides a method for detecting longitudinal forming line defects of an annealed steel plate for stamping, which is characterized by comprising the following steps of: preparing a sample, namely obtaining a produced steel coil as a sample from an annealing unit or a recoiling unit, obtaining a plurality of comparison samples with the same specification from a plate width sample, and marking material numbers; sample stretching: carrying out single stretching on the comparison samples, and increasing the stretching proportions of the plurality of comparison samples; polishing detection: polishing the sample along the length direction by using a polishing material; and defect judgment: detecting the polished sample. According to the method, the longitudinal forming stripe defects can be effectively detected in the mode that the cold-rolled annealed plate is uniaxially stretched and then polished, a powerful basis is provided for outflow prevention work of the longitudinal forming stripe defects, and the stability and market competition of products of iron and steel enterprises are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of defect inspection of plate steel products, and in particular to a method for detecting longitudinal forming line defects of annealed steel plates for stamping. Background Art

[0002] With the rapid development of the current automobile industry, automobile factories have gradually tightened their requirements for the use of exterior panels. The longitudinal forming stripe defect on the surface is a type of defect that is very easy to produce in cold-rolled annealed plates. This type of defect has no intuitive performance in the products off the steel plant. It will only appear on the surface of the parts after the user has stamped them. Therefore, the detection of longitudinal forming stripe defects is very easy to leak to users. Automobile manufacturers discover such defects during polishing after stamping. At this time, it not only seriously affects the production rhythm of users, but also brings certain economic losses and loss of product reputation to steel companies. Summary of the invention

[0003] The present disclosure aims to solve at least one of the technical problems existing in the prior art or related art.

[0004] To this end, the present disclosure provides a method for detecting longitudinal forming line defects of annealed steel plates for stamping, comprising the following steps:

[0005] Sample preparation: take the finished steel coils from the annealing unit or rewinding unit as the samples, take multiple comparison samples of the same specifications from the samples, and mark the material numbers;

[0006] Sample stretching: the comparative sample is subjected to unidirectional stretching, and the stretching ratios of the multiple comparative samples are increased;

[0007] Grinding test: use grinding materials to grind along the length of the sample;

[0008] Defect determination is based on testing the polished samples.

[0009] In a feasible implementation, the plurality of comparison samples include an original plate sample, a first comparison sample, a second comparison sample and a third comparison sample, and the stretching ratios of the first comparison sample, the second comparison sample and the third comparison sample are increased.

[0010] In a feasible implementation, the stretching ratio of the first comparative sample is set to 3.8% to 4.2%, the stretching ratio of the second comparative sample is set to 5.8% to 6.2%, and the stretching ratio of the third comparative sample is set to 7.8% to 8.2%.

[0011] In a feasible implementation manner, the stretching ratio of the first comparative sample is set to 4%, the stretching ratio of the second comparative sample is set to 6%, and the stretching ratio of the third comparative sample is set to 8%.

[0012] In a feasible implementation manner, the original plate sample, the first comparison sample, the second comparison sample and the third comparison sample are configured as long strip plates with a width direction*rolling direction of 400 mm*80 mm.

[0013] In a feasible implementation manner, the sample size is obtained on an annealing unit or a re-coiling unit and is set to 400 mm*plate width.

[0014] In a feasible implementation manner, the grinding material is an oil stone and / or a gauze.

[0015] In a feasible implementation manner, in the defect determination step, any one of the plurality of comparison samples that does not meet the qualification standard is considered unqualified.

[0016] In a feasible implementation, in the defect determination step, the determination criterion is to test the comparison sample after grinding, and if the detection stripes are clearly visible, it is unqualified; if the surface texture is uniform and there are no fine line stripes, it is qualified.

[0017] In a feasible implementation manner, in the grinding detection step, the grinding direction of the comparison sample is perpendicular to the rolling direction.

[0018] Compared with the prior art, the present disclosure includes at least the following beneficial effects: the present disclosure can effectively detect longitudinal forming stripe defects by grinding the cold-rolled annealed plate after unidirectional stretching, provide a strong basis for preventing the outflow of longitudinal forming stripe defects, and improve the stability and market competitiveness of steel enterprises' products. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present disclosure and, together with the description, serve to explain the principles of the present disclosure.

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0021] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the exemplary embodiments below. The accompanying drawings are only for the purpose of illustrating exemplary embodiments and are not to be considered as limiting the present application. Also, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0022] Figure 1It is a schematic diagram of the grinding direction disclosed in the present invention.

[0023] in, Figure 1 The corresponding relationship between the reference numerals and the component names is: 2-first comparative sample; 3-second comparative sample; 4-third comparative sample. DETAILED DESCRIPTION

[0024] In order to more clearly understand the above-mentioned objectives, features and advantages of the present disclosure, the scheme of the present disclosure will be further described below. It should be noted that the embodiments of the present disclosure and the features in the embodiments can be combined with each other without conflict.

[0025] In the following description, many specific details are set forth to facilitate a full understanding of the present disclosure, but the present disclosure may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present disclosure, rather than all of the embodiments.

[0026] With the rapid development of the current automobile industry, automobile factories have gradually tightened their requirements for the use of exterior panels. The longitudinal forming stripe defect on the surface is a type of defect that is very easy to produce in cold-rolled annealed plates. This type of defect has no intuitive performance in the products off the steel plant. It will only appear on the surface of the parts after the user has stamped them. Therefore, the detection of longitudinal forming stripe defects is very easy to leak to users. Automobile manufacturers discover such defects during polishing after stamping. At this time, it not only seriously affects the production rhythm of users, but also brings certain economic losses and loss of product reputation to steel companies.

[0027] Based on this, the embodiment of the present disclosure provides a method for detecting longitudinal forming stripe defects in annealed steel plates for stamping. The longitudinal forming stripe defects can be effectively detected by grinding the cold-rolled annealed plates after uniaxial stretching, providing a strong basis for preventing the outflow of longitudinal forming stripe defects and improving the stability and market competitiveness of steel enterprises' products.

[0028] The following is a detailed description of the method for detecting the longitudinal forming line defects of the annealed steel plate for stamping by using a specific embodiment:

[0029] Reference Figure 1 As shown, the present disclosure provides a method for detecting longitudinal forming line defects of annealed steel plates for stamping, comprising the following steps:

[0030] Sample preparation: The steel coils produced by the continuous annealing unit can be obtained from the annealing unit or the rewinding unit as samples. Multiple comparison samples with the same specifications are obtained from the samples, and the material numbers are marked for subsequent identification. During the process, care should be taken to protect the surface of the sample from scratches, rubbing marks and other obvious defects. Optionally, the sample size obtained on the annealing unit or the rewinding unit is set to 400mm*plate width, which is suitable for cold-rolled annealed steel plates with a strip width of ≥400mm. Other strips of different sizes can be selected according to the actual size. It should be noted that when selecting the comparison sample steel, an integer value must be selected to meet the stretching requirements. On the premise of meeting the stretching requirements, stability can also be taken into account. Plate widths that are too long or too short are not conducive to single-item stretching.

[0031] Sample stretching: The comparison sample is stretched in a single item, and the stretching ratio of multiple comparison samples is increased gradually, so as to analyze whether it meets the stamping requirements of automobile companies under various stretching conditions.

[0032] For grinding inspection, use grinding materials to grind along the length direction of the sample. The grinding direction of the specific comparison sample is perpendicular to the rolling direction. The grinding material can be oil stone or gauze. The pressure is uniform during the grinding process and the entire board surface is polished. The pressure is uniform during the grinding process and the entire board surface is polished.

[0033] Defect determination is based on testing the polished samples.

[0034] In some embodiments, the plurality of comparative samples include an original plate sample, a first comparative sample 2 , a second comparative sample 3 , and a third comparative sample 4 , and the stretching ratios of the first comparative sample 2 , the second comparative sample 3 , and the third comparative sample 4 are increased.

[0035] In this embodiment, the comparison samples are divided into four groups, namely, four progressive stretching ratios, one of which is set as an original plate sample, that is, a sample that is not subjected to single-item stretching. Taking the original plate sample as a benchmark, the remaining first comparison sample 2, second comparison sample 3 and third comparison sample 4 are stretched in progressive ratios to fully reflect the state under each stretching ratio.

[0036] In some embodiments, the stretching ratio of the first comparative sample 2 is set to 3.8% to 4.2%, the stretching ratio of the second comparative sample 3 is set to 5.8% to 6.2%, and the stretching ratio of the third comparative sample 4 is set to 7.8% to 8.2%.

[0037] In this embodiment, the stretching ratio of the first comparative sample 2 is set to 3.8% to 4.2%, and the preferred stretching ratio is 4%. When the stretching ratio is lower than 3.8%, it cannot meet the stamping requirements of automobile enterprises and has no reference value; the stretching ratio of the second comparative sample 3 is set to 5.8% to 6.2%, preferably 6%. When the stretching ratio is lower than 5.8%, it conflicts with the upper limit of the first comparative sample 2. The two stretching ratios have errors within this range and have no reference value. The stretching ratio of the third comparative sample 4 is set to 7.8% to 8.2%, preferably 8%. Within the above ratio range, the stamping requirements of automobile enterprises can be best simulated, and the stretching stability is low outside the range of less than 3.8% and higher than 8.2%. In the field of steel coils produced by continuous annealing units, due to the particularity of steel materials, the stretching ratio range of higher than 8.2% or lower than 3.8% will produce a "false pass", but in fact it does not meet the requirements.

[0038] In some embodiments, the original plate sample 1, the first comparison sample 2, the second comparison sample 3 and the third comparison sample 4 are set as long strips of 400mm*80mm in the width direction*rolling direction. After stretching at ratios of 4%, 6% and 8% respectively, the lengths after stretching are 416mm, 424mm and 432mm respectively.

[0039] In some embodiments, in the defect determination step, any one of the multiple comparison samples that does not meet the qualified standard is unqualified. In the defect determination step, the judgment standard is based on the inspection of the polished comparison sample. If the detection stripes are clearly visible, it is unqualified; if the surface texture is uniform and there are no fine line stripes, it is qualified. Further, when inspecting the clarity of the stripes, the staff can directly judge with the naked eye, but the error of the qualified rate of this judgment method is large. Specifically, electronic observation can be used to make the judgment together.

[0040] In the present disclosure, the terms "first", "second", and "third" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance; the term "plurality" refers to two or more, unless otherwise expressly defined. The terms "installed", "connected", "connected", "fixed", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; "connected" can be a direct connection or an indirect connection through an intermediate medium. For those of ordinary skill in the art, the specific meanings of the above terms in the present disclosure can be understood according to the specific circumstances.

[0041] In the description of the present disclosure, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "left", "right", "front", "back", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, rather than indicating or implying that the device or unit referred to must have a specific direction, be constructed and operated in a specific orientation, and therefore, should not be understood as a limitation on the present disclosure.

[0042] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0043] The above are only preferred embodiments of the present disclosure and are not intended to limit the present disclosure. For those skilled in the art, the present disclosure may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present disclosure shall be included in the protection scope of the present disclosure.

Claims

1. A method for detecting longitudinal forming line defects of annealed steel sheet for stamping, characterized in that: The steps include: Sample preparation: take the finished steel coils from the annealing unit or re-coiling unit as the samples, take multiple comparison samples of the same specifications from the samples, and mark the material numbers; Sample stretching: the comparative sample is subjected to unidirectional stretching, and the stretching ratios of the multiple comparative samples are increased; Grinding test: use grinding materials to grind along the length of the sample; Defect determination is based on testing the polished samples.

2. The method for detecting longitudinal forming line defects of annealed steel sheet for stamping according to claim 1, characterized in that: The plurality of comparative samples include an original plate sample, a first comparative sample, a second comparative sample and a third comparative sample, and the stretching ratios of the first comparative sample, the second comparative sample and the third comparative sample are increased.

3. The method for detecting longitudinal forming line defects of annealed steel sheet for stamping according to claim 2, characterized in that: The stretching ratio of the first comparative sample is set to 3.8% to 4.2%, the stretching ratio of the second comparative sample is set to 5.8% to 6.2%, and the stretching ratio of the third comparative sample is set to 7.8% to 8.2%.

4. The method for detecting longitudinal forming line defects of annealed steel sheet for stamping according to claim 3, characterized in that: The stretching ratio of the first comparative sample is set to 4%, the stretching ratio of the second comparative sample is set to 6%, and the stretching ratio of the third comparative sample is set to 8%.

5. The method for detecting longitudinal forming line defects of annealed steel sheet for stamping according to claim 1, characterized in that: The original plate sample, the first comparison sample, the second comparison sample and the third comparison sample are set as long strip plates with a width direction*rolling direction of 400 mm*80 mm.

6. The method for detecting longitudinal forming line defects of annealed steel sheet for stamping according to claim 1, characterized in that: The sample size is obtained on the annealing unit or the rewinding unit and is set to 400 mm*plate width.

7. The method for detecting longitudinal forming line defects of annealed steel sheet for stamping according to claim 1, characterized in that: The grinding material is oil stone and / or gauze.

8. The method for detecting longitudinal forming line defects of annealed steel sheet for stamping according to claim 1, characterized in that: In the defect determination step, any one of the plurality of comparison samples that does not meet the qualification standard is considered unqualified.

9. The method for detecting longitudinal forming line defects of annealed steel sheet for stamping according to claim 1, characterized in that: In the defect determination step, the determination criteria are as follows: if the comparison sample is tested after grinding, it is unqualified if the detection stripes are clearly visible; if the surface texture is uniform and there are no fine line stripes, it is qualified.