Hybrid chemical-physical vapor deposition process for synthesizing environmental barrier coatings

Through a hybrid chemical/physical vapor deposition method, combined with plasma activation technology, the problems of deposition uniformity and material oxidation of SiC-based ceramic composite coatings at low temperatures are solved, achieving efficient environmental barrier coating deposition and improving the material's durability. Mechanical properties and stability.

CN118829622APending Publication Date: 2024-10-22OERLIKON SURFACE SOLUTIONS AG PFAFFIKON
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202280080349.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-11-30
Filing Date
2022-11-30
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

When the existing technology deposits environmental barrier coatings of SiC-based ceramic composite materials, it is difficult to achieve uniform thickness and microstructure control at low temperatures, and high deposition temperatures can cause oxidation of the material and reduce mechanical properties.

Method used

Using a hybrid chemical/physical vapor deposition method, combining plasma-activated chemical vapor deposition and physical vapor deposition, the deposition of Si bonding coating and Yb-Si-O barrier coating at low temperature is achieved through plasma pretreatment and arc discharge. , ensuring interface clarity and coating integrity.

Benefits of technology

Depositing a complete environmental barrier coating at relatively low temperature improves the corrosion resistance and water vapor stability of the coating, reduces the oxidation risk of the material, and enhances the mechanical properties of SiC-based CMC materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118829622A_ABST
    Figure CN118829622A_ABST
Patent Text Reader

Abstract

Manufacturing methods for synthesizing environmental barrier coating systems (EBCs) that protect Si-based ceramic matrix composite (CMC) materials from oxidation and volatilization at elevated temperatures are disclosed. The method of manufacture is performed in vacuum and includes the step of depositing a silicon bond coating and an oxygen-containing barrier coating. The method is supported by plasma, preferably by arc discharge, which results in complete dissociation of a gas precursor, such as silane. Plasma is also used to pre-treat a substrate in an uninterrupted process chain. Deposition systems with substantially vacuum and plasma components and EBC coatings made by the methods are disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Scope of the Invention

[0001] The present invention relates to deposition techniques and methods for synthesizing environmental barrier coatings (EBCs) that protect Si-based ceramic matrix composite (CMC) materials from oxidation and volatilization at high temperatures. background

[0002] Silicon carbide (SiC) and silicon nitride based ceramic matrix composite (CMC) materials (both summarized herein under "Si-based CMC materials") are the materials of choice for hot zones in next generation gas turbine engines due to their high specific strength and high temperature stability. However, CMCs undergo rapid recession in water vapor environments, resulting in reduced mechanical strength and structural integrity of the CMC components. Therefore, Si-based CMCs need to be protected by ceramic environmental barrier coatings (EBCs) to prevent surface degradation of these CMC materials. The approach to coating design is based on a combination of a bond coat (adhesion layer) and a chemical barrier that is specific to a specific Si-based material. For SiC-based materials, some combinations consisting of a bond coat and a barrier layer have been studied in the past. A promising EBC system consists of a silicon bond coat applied to a substrate followed by a rare earth silicate protective coating. Among the rare earth silicates, Yb2Si2O7 appears to be the most promising candidate due to its low degradation rate in water vapor containing environments, excellent phase stability up to its melting temperature of 1850°C, and a coefficient of thermal expansion (CTE) that is reasonably well matched to the silicon-based CMC substrate.

[0003] There are different methods to deposit such coatings onto SiC based components used in the hot zone of a gas turbine.

[0004] Air plasma spraying (APS) has been widely used for dense EBC deposition. The advantages of this technology are low cost, high deposition rate and wide composition flexibility. However, the APS method is challenging when coating complex-shaped engine components such as blades and impellers because variations in spray distance and spray angle will result in uneven coating microstructure and thickness. In addition, controlling the interface and specific nucleation processes in APS multilayer coatings can be difficult due to deposition under atmospheric conditions. Therefore, new process methods for EBC deposition for different engine component applications are needed, which allow better control of coating microstructure and properties.

[0005] In US 2020 / 0039892A1, chemical vapor deposition (CVD) is described for depositing a silicon bonding coating as part of an EBC coating. The method is implemented at a deposition pressure in the range of about 115 torr to about 150 torr, which is equivalent to a range of about 15,300 Pa to about 20,000 Pa, and uses a silicon-containing precursor. However, in order to dissociate the precursor and obtain a crystalline Si coating deposition, the required deposition temperature is higher than 900°C, with a substrate temperature of about 1100°C being preferred. High deposition temperatures can cause oxidation of the SiC / SiC CMC substrate and degrade its mechanical properties. Purpose of the Invention

[0006] In the present invention, a hybrid chemical / physical vapor phase method for EBC coating deposition is developed. A typical EBC coating consists of Figure 1 The layer stack shown in is composed. The hybrid CVD / PVD method allows the deposition of a complete EBC layer stack at a relatively low deposition temperature without interruption of vacuum. The coating includes a Si bonding coating and a Yb-Si-O top coating, and may include additional coatings. Figure 1 show: 1 Si-based CMC substrate 2 to the interface of silicon bonding coating (optional) 3a, 3b Silicon bond coatings which may have variations in morphology (e.g., particle size) or composition (e.g., incorporation of dopants) within the bond coating 4 A transition layer to a barrier coating (e.g., silicate), which may be different in composition and structure from the bond coating and / or the barrier coating 5 Barrier coating, here as an example is Yb-Si-O 6 Top coating, which is used to improve the performance of the barrier coating, i.e. in terms of corrosion resistance, water vapor stability, CMAS resistance, etc. (optional) Description of the invention

[0007] Below, reference Figure 1 The invention is described with respect to a specific layer stack. This description is intended only as an example and should not be construed as limiting the broader scope of the invention.

[0008] The present invention uses a combination of plasma-activated chemical vapor deposition (CVD) and physical vapor deposition (PVD) methods for EBC deposition. Activation of vapor in a plasma is a method that enables coating deposition at much lower temperatures than conventional CVD. This is significantly different from conventional chemical vapor deposition such as that used in patent application US 2020 / 0039892 A1.

[0009] For a better understanding between the prior art and the method of the present invention, refer to Figure 2 For depositing silicon bonding coatings and reference Figure 5 The sequence of process steps is explained for a complete EBC. Fig.10 In FIG. 1 , a schematic diagram of a deposition system is given, which allows the deposition of EBCs using the method of the present invention.

[0010] In the case of EBC layer systems, the silicon bond coat is a Si layer that exhibits excellent chemical and bonding compatibility with the CMC surface. In addition, the silicon bond coat should have a coefficient of thermal expansion (CTE) close to that of the CMC substrate. The silicon bond coat is typically a homogeneous layer that may also contain alloying elements other than Si.

[0011] Reference now Figure 2 Deposition of a silicon bonding coating is explained. The method 100 includes the following steps: substrate loading 101, pumping the deposition chamber 102, heating the substrate to a desired temperature 103, pre-treating the substrate by plasma 104, initiating a gas arc discharge and a silicon precursor 105, optionally doping from a gas source or a solid source 106, depositing a silicon bonding coating 107, cooling the system 108, and exhausting and unloading the substrate 109. Steps 103 to 107 are process steps utilizing plasma 110.

[0012] A pretreatment step 104 is introduced to clean the substrate and remove the native oxide on the substrate. In addition to the plasma helping to reduce the deposition temperature, the plasma plays an important role in the pretreatment of the silicon-based substrate. The native oxide at the surface of the Si-based substrate can hinder the good adhesion of the silicon-bonded coating later, and therefore needs to be removed. The removal of the native oxide is carried out by plasma activation of a reactive gas used to reduce the oxide and form volatile compounds (which are pumped away by the pump) with oxygen. Producing atomic or ionized hydrogen by hydrogen discharge is an example of such a reactive surface pretreatment or cleaning. Here, argon / hydrogen discharge is used, which has a discharge current of 200A, a discharge voltage of 50V, an argon flow rate of 60sccm (standard cubic centimeters per minute) and a hydrogen flow rate of 300sccm. In such a process, loose carbon pollutants are also volatilized. The typical thickness of these oxides or carbon pollutants is on the order of 10nm.

[0013] As is known to those skilled in the art of vacuum deposition technology, exposing a pre-cleaned substrate surface to the environment will lead to immediate re-contamination of the pre-treated substrate surface, since such a pre-treated surface is highly reactive with the gases in the ambient atmosphere. Therefore, there must be a direct transition to the next process step of depositing the EBC, i.e. the silicon-bonding coating, without vacuum interruption. All of this, i.e. surface pre-treatment, cleaning and a controlled vacuum environment ensures better control of the nucleation process of the silicon-bonding coating on the Si-based substrate and, therefore, better formation of the interface.

[0014] The formation of the interface Figure 3 As shown in , it shows a silicon bonding coating synthesized using the method of the present invention. Figure 3 A silicon-bonded coating with a thickness of 3 μm deposited from a silane precursor (SiH4) is shown. Dissociation and activation of the silane was achieved by arc discharge in an argon working gas with an Ar flow of 80 sccm and an arc discharge current of 120 A and an arc voltage of 75 V. A silane flow of 250 sccm was used. The substrate temperature during deposition was 550°C. Figure 3 A cross section of a silicon coating at a silicon carbide substrate obtained by transmission electron microscopy (TEM) is shown. The interface consists of a nucleation zone with a thickness of about 200 nm, and after this nucleation zone, a transition to columnar growth is visible, which shows that the method of the present invention can achieve columnar growth of silicon at already low temperatures. The Si coating ( Figure 3 ) has a segmented strain-resistant microstructure.

[0015] In the context of the present invention, vacuum is understood to be less than 1×10 3 Pa but not less than 1×10 -6 Pa pressure. Most preferably, the pressure is between 100Pa and 0.001Pa. 3 Pa pressure increases the risk of contamination, but below 1×10 -6 The pressure of Pa spans to the ultra-high vacuum range, where special materials and equipment, such as vacuum pumps, are required.

[0016] Cross-sectional micrographs of silicon bond coatings deposited on SiC substrates obtained by TEM show that columnar growth can be achieved and that the plasma treatment of the present invention is a suitable technique for controlling the nucleation and growth of silicon bond coatings at low temperatures.

[0017] The excellent adhesion of the silicon bond coating to the substrate is characterized by the formation of dislocations in the substrate surface. Figure 4 . A bright field (BF) TEM cross section shows the interface between the SiC substrate and the thin silicon bonding coating. The micrograph gives an impression of the good quality of the interface between the SiC and the silicon bonding coating. The interface is sharp and there is no visible porosity. The dislocations generated in the SiC substrate by the silicon bonding coating after annealing demonstrate the excellent adhesion and stability of the SiC-Si interface. With reference to the above description, the interface is formed in a vacuum process sequence consisting of plasma treatment of the SiC surface at a substrate temperature of about 550°C and re-deposition of the silicon bonding coating in a plasma environment without interruption of the vacuum.

[0018] Another feature of the method of the present invention is to use arc discharge to dissociate the gas precursor, in this example, silane. The high electron current density of the arc discharge (typical parameters of such a discharge are 20A to 1000A at a voltage between 15V and 100V) leads to complete dissociation of the precursor. This means that about 100% of the Si fed into the system with the precursor will react in the chamber. This is different from other types of plasma-enhanced CVD methods, in which some amount of unreacted Si-containing (silicon-containing) precursors are pumped away. Complete dissociation also produces a silicon coating that does not contain hydrogen or only shows very little hydrogen content in the initially deposited silicon bonding coating. This strongly contributes to the stability of the silicon bonding coating at high temperatures because hydrogen contributes to instability. The hydrogen content in the silicon bonding coating is measured by elastic recoil detection and is less than 5at.%, typically even less than 3at.%. Importantly, these characteristics of the method of the present invention are achieved at medium and low substrate temperatures below 600°C.

[0019] The deposition of the silicon-bonding coating is achieved by plasma activation and dissociation of a silicon-containing precursor. A variety of silicon-containing gases can be used as silicon-containing precursors and may contain one or more of the following chemicals: silane, disilane, dichlorosilane, trichlorosilane, silicon tetrachloride, methylsilane, silicon tetrafluoride, trimethylsilane, tetramethylsilane, hexachlorodisilane, etc. The typical flow rate of the silicon-containing precursor gas is 1 sccm to 101 / m, preferably between 10 sccm and 11 / m. In the following experiments, silane was used as a precursor. In order to activate the precursor, an arc discharge is used. The arc discharge is characterized by an electron current between 10A and 400A and a discharge voltage between 15V and 100V. The arc discharge can be generated by a discharge in a rare gas such as argon or by cathode arc evaporation of a metal target. The high electron current of the arc discharge is very effective for the dissociation of the silicon-containing precursor. This is a pretreatment for synthesizing silicon-bonding coatings at a substrate temperature below 600°C at a high deposition rate. The degree of utilization of the silicon in the precursor is determined as the ratio of silicon atoms deposited in the chamber to silicon atoms fed into the chamber by the precursor. The degree of utilization according to the method of the invention is higher than 80%, preferably higher than 90%. Due to the very efficient dissociation of the silicon-containing precursor enhanced by the argon plasma gas, the coating deposition rate shows almost no dependence on the substrate temperature in the range between 300° C. and 600° C. This is an advantage over conventional thermal CVD techniques, in which the substrate temperature has a major influence on the deposition rate.

[0020] Another advantage of the method of the present invention is that plasma-activated deposition can be combined with additional doping sources. As an example, in order to dope the silicon bond with another element, the process technology allows the silicon-containing precursor to be run together with another gaseous precursor, such as a carbon-containing or boron-containing precursor or a combination of these. In addition, the method of the present invention also allows simultaneous evaporation from a combination of a silicon-containing precursor and a solid source. The solid source can especially be the volatilization of a metal or semimetal by cathodic arc evaporation or sputtering. As an example, using the above-mentioned process parameters for silicon bond coating deposition, an additional sputtering source with an aluminum target can be triggered, resulting in the doping of the silicon bond coating by aluminum. Other targets for sputtering or cathodic arc evaporation can also be used to dope the silicon bond coating with suitable elements. Chemical substances containing one or more of the following elements can be incorporated into the silicon bond coating: Al, B, C, O, N, Ga, In, P, Li, Na, K, Ca, Mg, Sr, Ba.

[0021] exist Figure 2 In the figure, all plasma-enhanced process steps are outlined with dashed lines. It can be seen that all plasma-based steps are performed without interruption of the vacuum, i.e. in the entire process chain from substrate loading until venting of the deposition system after completion of the silicon bonding coating deposition. Uninterrupted vacuum processes have the advantage of reduced contamination compared to processes in which the vacuum is interrupted.

[0022] In addition to substrate pretreatment and deposition of the silicon bonding coating, the method of the invention also includes the synthesis of a complete EBC layer stack. In the method of the invention, this complete process sequence is also achieved in one process, i.e. without vacuum interruption. This Figure 5 The process sequence shown in is shown in . The deposition of the complete EBC coating system includes substrate pretreatment and deposition of a silicon bond coat and deposition of a barrier top coat. In its simplest form, the deposition of the barrier top coat is performed directly after the deposition of the silicon bond coat. However, if additional adaptability is required between the silicon bond coat and the barrier coat, for example for the purpose of enhancing the water vapor / oxygen diffusion barrier, additional layers may be incorporated. The process sequence 200 generally includes the following steps: loading the SiC-CMC substrate 201, pumping the deposition chamber 202, heating the substrate to a moderate temperature 203, pretreating the substrate by plasma 204, initiating a gas arc discharge and a silicon precursor 205, depositing a silicon bond coat 206, initiating a cathodic arc discharge of a Me target 207, initiating a silicon precursor (optional) and oxygen 208, depositing a Me-Si-O barrier coating 209, cooling the system 210, and exhausting and unloading the SiC-CMC with EBC 211. In Figure 5In FIG. 1 , all plasma-based process steps 203 to 209 are outlined by dashed lines 212. As can be seen, all plasma-based steps are performed without interruption of the vacuum. Thus, the vacuum is not interrupted from the step of substrate loading until the deposition system is vented after the entire EBC layer stack is completed.

[0023] In an EBC coating system, the barrier coating acts as a chemical barrier between the silicon bond coat and the barrier coating or top coat. The barrier coating should avoid potential chemical reactions that would damage the EBC. The barrier coating should protect the bond coat from oxidation and ideally should resist water vapor attack.

[0024] Figure 6 A first embodiment of a complete EBC layer stack according to the method of the present invention is shown, which consists of a SiC substrate, a silicon bonding coating and an Al-Si-O barrier coating. In this embodiment, a silicon bonding coating with a thickness of 29 μm is deposited on a pretreated SiC substrate using a silane source. Silane is activated and dissociated in an arc discharge for silicon bonding coating synthesis. The arc discharge current is 120A, the discharge voltage is 75V, the argon flow rate is 80sccm, and the silane flow rate is 250sccm. After the silicon bonding coating is deposited, cathodic arc evaporation using an aluminum target as a cathode is initiated, which uses an arc current of 145A, oxygen with a flow rate of 220sccm, and silane with a flow rate of 66 is added to the discharge. The deposition temperature is 550°C. Using these parameters, 30μmAl-Si-O is deposited as Al 35 Si5O 60 In this deposition, the Al content of the coating is controlled by the evaporation rate from the Al target, and the Si content of the coating is controlled by the flow rate of the silane precursor. The oxygen flow rate is adjusted to achieve complete oxidation of Al-Si-O. Figure 6 The coating is shown after annealing at 1400° C. The interface is sharp and no porosity is formed between the silicon bond coating and SiC and between the silicon bond coating and the Al—Si—O barrier coating.

[0025] Figure 7 Another example of a coating system prepared by the method of the present invention is given in FIG. The figure shows an EBC layer stack consisting of a silicon binder coating and a dense Yb-Si-O barrier coating deposited on a SiC substrate. The figure shows a TEM cross-section of the as-deposited layer stack. The interface is sharp and there is no porosity, indicating good coating adhesion. A few droplets (probably defects during the deposition of the silicon binder coating) and droplets from cathodic arc evaporation are visible in the cross-section. These droplets and defects are not considered critical to the functionality of the coating system and usually disappear during annealing (will be in Figure 8). The substrate surface was pretreated by reactive plasma and a 3 μm thin silicon bonding coating was deposited in an argon arc discharge with a discharge current of 120 A and a discharge voltage of 75 V using an argon flow rate of 80 sccm and a silane flow rate of 250 sccm. After the silicon bonding coating was deposited, ytterbium was evaporated from an elemental ytterbium target, which was used as a cathode in cathodic arc evaporation. An arc current of 120 A was used to evaporate the ytterbium (Yb) target, and a silane flow rate of 200 sccm and an oxygen flow rate of 400 sccm were used to synthesize a Yb-Si-O barrier coating. The deposition temperature was 550° C. As a result, Yb was synthesized. 29 Si 11 O 59 Barrier coating (measured by EDX). The complete process sequence is carried out without interruption of the vacuum, i.e. in one continuous process sequence.

[0026] Figure 8 After annealing at 1400°C Figure 7 Layer stacking afterwards. The interface is still stable and flat, and no porosity is formed. In the silicon bond coating, columnar structures are visible, and a thin (about 300 nm) and dense silicon oxide is formed on top of the silicon bond coating. Between silicon oxide and the Yb-Si-O barrier coating, a thin (about 200 nm) transition can be identified.

[0027] Another embodiment of the present invention is Fig. 9 , a complete EBC layer stack having a silicon bonding coating of ˜30 μm and a Yb-Si-O barrier coating of ˜12 μm is deposited on a SiC substrate. The Yb-Si-O coating comprises ˜77 vol % Yb2Si2O7 and ˜23 vol % Yb2SiO5 phases. This demonstrates the flexibility of the method of the present invention for depositing EBCs having various chemistries. The combination of Yb2Si2O7 and Yb2SiO5 phases is advantageous for obtaining a barrier coating having a low corrosion rate and a thermal expansion coefficient that is well matched to the CMC substrate. The Yb2SiO5 phase has a particularly low degradation rate (sometimes referred to as corrosion rate) in an environment containing water vapor, but has a thermal expansion coefficient that is not well matched to the SiC / SiC CMC substrate. On the other hand, the phase Yb2Si2O7 has a thermal expansion coefficient that is well matched to the SiC / SiC CMC substrate, but has a higher degradation rate than the Yb2SiO5 phase. The synthesis of barrier coatings containing both Yb2Si2O7 and Yb2SiO5 phases allows for a technologically efficient combination of these two properties.

[0028] In another aspect of the invention, the coating method can be used to prepare a barrier coating comprising a combination of one or more Yb-Si-O phases and at least one second type phase that does not contain Yb. The combination of Yb-Si-O and the second type phase allows the thermal expansion coefficient to be customized for different substrates and coatings. The second type phase can be Al2O3, an alkali metal oxide, or an alkaline earth metal oxide. In particular, Yb2Si2O7 or Yb2SiO5 can be combined with Al2O3, an alkali metal oxide, or an alkaline earth metal oxide.

[0029] The proposed EBC layer stack demonstrates the capability of the method of the present invention to manufacture such a structure in one process sequence. Fig.10 A schematic diagram of a deposition system for such a process sequence is given.

[0030] Fig.10 Combinations of gas sources for working gases such as argon and for reactive gases such as oxygen, nitrogen, hydrocarbons and for Si-containing precursors are shown. These sources can be operated alone or in combination with solid sources such as cathode arc sources and sputtering sources. A very important feature of the process is the use of plasma. This includes surface pretreatment, which defines reliable conditions for the deposition of silicon-bonding coatings, which helps to produce strain-resistant columnar structures. In the synthesis of silicon-bonding coatings, almost complete dissociation of silicon-containing precursors in the arc discharge is important. It helps to avoid the incorporation of hydrogen in the silicon-bonding coating at low deposition temperatures below 600°C. The optional incorporation of dopants during silicon growth and the simple addition of additional gas sources or solid sources in this deposition step contribute to the versatility of the method of the present invention. Plasma enhancement by arc discharge is the key to independently control the deposition rate of silicon-containing precursors at deposition temperatures between 300°C and 600°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 : Schematic representation of a layer stack deposited by the method of the invention. The entire layer stack (bond coating and barrier coating as well as all further interface coatings) is deposited without interruption of the process vacuum, ie in one process sequence and in a plasma environment.

[0032] Figure 2 : Sequence of process steps for depositing a silicon bonding coating according to the method of the present invention

[0033] Figure 3 : TEM cross-sectional micrographs from a silicon bond coating with columnar morphology showing column widths between 10 nm and 50 nm.

[0034] Figure 4 : BF-TEM cross section of the SiC-silicon bonding coating interface after annealing at 1400°C, where dislocations are formed in the SiC substrate.

[0035] Figure 5 : Example of a process sequence for depositing a complete EBC layer stack consisting of SiC pretreatment / silicon bond coating / barrier coating.

[0036] Figure 6 : SiC-silicon bond coating annealed at 1400℃-Al 35 Si5O 60 Scanning electron microscope (SEM) cross-sectional micrograph of a layer stack.

[0037] Figure 7 : TEM cross section of a SiC substrate with a silicon bond coating (3 μm) and a Yb-Si-O barrier coating (6 μm).

[0038] Figure 8 : TEM cross section of a SiC substrate with a silicon bond coating (3 μm) and a Yb—Si—O barrier coating (6 μm) after annealing at 1400°C.

[0039] Fig. 9 : SEM image of as-deposited Yb-Si-O / Si EBC using hybrid vapor deposition method

[0040] Fig.10 : Schematic diagram of a deposition system for a hybrid PVD / CVD method including a process sequence for substrate pretreatment, deposition of a silicon bond coating and a barrier coating. List of Reference Numerals 1. Substrate 2 to the interface of the bonding coating (optional) 3a Bonding coating 3b Bond coatings that may have variations in morphology (e.g., particle size) or composition (e.g., incorporation of doping elements) 4 Transition layer to barrier coating (e.g. silicate), which may be different in composition and structure from the bond coating and / or barrier coating 5. Barrier coating 6 Optional top coating, which is used to improve the performance of the barrier coating, such as in terms of corrosion resistance, water vapor stability, CMAS resistance, etc. 11Vacuum deposition chamber 12 Pumping System 13 Door for loading substrate 14 Gas arc discharge sources (multiple) 15 cathode arc sources (multiple) 16 Sputtering sources (multiple) 17 Operating gas inlet for gas arc discharge (multiple) 18 Gas inlet for reactive gases (multiple) 19 Gas inlet containing Si precursor 20Substrate holder with substrate bias 21 Substrate heater 100Process sequence for depositing silicon bond coating 101 Substrate Loading 102 Pumping Deposition Chamber 103Heating the substrate to the desired temperature 104 Pre-treating the substrate by plasma 105 Initiation of gas arc discharge and silicon precursor 106 Doping from gaseous or solid sources (optional) 107 Deposition of Silicon Bond Coating 108 Cooling System 109 Exhaust and unload substrate 110Process steps using plasma 200 Process sequence for depositing a complete EBC layer stack 201 Loading SiC-CMC substrate 202 Pumping Deposition Chamber 203 Heat the substrate to a medium temperature 204 Pre-treatment of substrate by plasma 205 Initiation Gas Arc Discharge and Silicon Precursor 206 Deposition of silicon bond coating 207 Initiates Cathodic Arc Discharge of Me Target 208 initiator silicon precursor (optional) and oxygen 209 Deposition of Me-Si-O barrier coating 210 Cooling System 211 Exhaust and unload SiC-CMC with EBC 212Process steps using plasma

Claims

1. A method for manufacturing an environmental barrier coating (EBC) system onto a substrate, comprising the step of depositing a silicon bonding coating, and at least one step of depositing an oxygen-containing barrier coating, Features The manufacturing method is carried out in a vacuum environment.

2. The method of claim 1, wherein the manufacturing method comprises at least one substrate pretreatment step, which is performed in a vacuum environment prior to the step of depositing the silicon bond coating.

3. The method according to claim 2, Features The at least one substrate pretreatment step and the step of depositing a silicon bond coating, and the at least one step of depositing an oxygen-containing barrier coating are part of a vacuum process with no interruption of vacuum during or between the process steps.

4. The method according to claim 1, 2 or 3, Features The vacuum environment includes plasma.

5. The method according to claim 4, Features The plasma environment is generated by at least one arc discharge, preferably in at least one noble gas, most preferably in argon.

6. The method according to claim 5, Features The at least one arc discharge is operated at a discharge current in the range of 20A to 1000A and a discharge voltage in the range of 15V to 100V.

7. The method according to claim 5, Features The at least one arc discharge is used to dissociate at least one silicon-containing precursor.

8. The method according to claim 1 or claim 4, Features The method is carried out at a temperature of the substrate below 600°C.

9. The method according to claim 1, Features The silicon bond coating is deposited to a thickness in the range between 0.01 μm and 500 μm.

10. The method according to claim 9, Features The silicon bond coat is oxidized after deposition.

11. The method according to claim 9, Features The silicon bond coat is doped by sputtering at least one doping element from at least one sputtering source.

12. The method of claim 11, wherein the at least one doping element is one or more elements selected from Al, B, C, O, N, Ga, In, P, Li, Na, K, Ca, Mg, Sr and Ba.

13. The method according to claim 1 or 4, Features The oxygen-containing barrier coating is produced by cathodic arc evaporation of at least one metal target, the metal target comprising Al or comprising at least one rare earth element.

14. The method according to claim 13, Features The arc evaporation is performed in an oxygen-containing environment.

15. The method according to claim 13, Features At least one silicon-containing precursor is introduced simultaneously with cathodic arc evaporation of the at least one metal target.

16. The method according to claim 15, Features The silicon precursor is introduced at a flow rate ranging from 1 sccm to 10 l / m, preferably at a flow rate ranging from 10 sccm to 1 l / m.

17. The method according to claim 13, 14 or 15, Features The oxygen-containing barrier coating comprises phase Yb 2 Si 2 O 7 and Yb 2 SiO 5 .

18. The method according to claim 13, 14 or 15, Features The oxygen-containing barrier coating comprises at least one Yb-Si-O phase and at least one second type phase, wherein the second type phase is Al 2 O 3 , at least one of an alkali metal oxide or an alkaline earth metal oxide.

19. The method according to claim 2, Features The pretreatment reduces the thickness of the surface oxide, in particular silicon oxide in case of Si-based substrates, to a thickness below 30 nm, preferably below 10 nm.

20. The method of claim 1, wherein the substrate consists of or comprises a ceramic matrix composite (CMC).

21. A deposition system for producing an environmental barrier coating using the method according to claim 1, Features The deposition system includes at least one vacuum deposition chamber, at least one pumping system, and at least one plasma source.

22. An environmental barrier coating system made according to claim 1, deposited on a substrate, Features The interface between the substrate and the silicon bond coating is sharp and free of porosity.

Citation Information

Patent Citations

  • Silicon Bond Coat With Columnar Grains and Methods of its Formation

    US20200039892A1

  • System and method for protection of high temperature machinery components

    CN102900472A

  • Coating system for a gas turbine component

    CN104428448A

  • Thermal / environment barrier coating based on ceramic composite material and preparation method of thermal / environment barrier coating

    CN109336647A

  • Vacuum Treatment Installation and Vacuum Treatment Method

    US20080292812A1