High-capacity superabsorbent material and preparation method thereof

Through staged polymerization technology and copolymerization of redox-active inorganic salts, a non-uniform microstructure and interpenetrating network are formed, which solves the problem of SAM salt sensitivity, improves absorption capacity and salt resistance, and realizes wider application potential.

CN118829670AActive Publication Date: 2024-10-22KIMBERLY CLARK WORLDWIDE INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202280092558.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-02-28
Publication Date
2024-10-22
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

Existing superabsorbent polymers (SAMs) exhibit salt sensitivity in environments with high salt content, resulting in reduced absorption capacity, and traditional solutions are costly and impractical.

Method used

Staged polymerization technology is used to copolymerize with selected redox-active inorganic salts to form a non-uniform microstructure and interpenetrating network that alleviates salt sensitivity and increases absorption capacity.

Benefits of technology

Significantly improve the absorption properties and salt resistance of SAM and reduce salt sensitivity, while maintaining good performance of other performance attributes, providing a wider application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118829670A_ABST
    Figure CN118829670A_ABST
Patent Text Reader

Abstract

Superabsorbent materials (SAMs) and methods of making SAMs are described herein. The superabsorbent material is copolymerized with a selected redox active inorganic salt during a staged polymerization process. The copolymer-based superabsorbent material has significantly improved absorption properties. The compositions and methods described herein can be used in a variety of absorbent products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to superabsorbent materials (SAMs) and methods for preparing SAMs. SAMs are copolymerized with selected redox-active inorganic salts in a staged polymerization process. Copolymer-based SAMs have significantly improved absorption properties. Compositions and methods according to the present disclosure can be used in a variety of absorbent products. Background Art

[0002] Superabsorbent polymer (SAP) is a three-dimensional network that can absorb and retain water (or other aqueous media) and physiological fluids such as urine and blood that exceed hundreds of times of its own dry weight, which usually depends on the ion concentration of the aqueous solution. SAP has applications in multiple fields, including medicine, personal care products, biomaterials, biosorbents and agriculture. The first commercial SAP was produced by the alkaline hydrolysis of starch-g-polyacrylonitrile in 1970. Although these polymers can absorb up to 500g / g of water, they are mechanically weak in their swollen state. SAP was developed for sanitary applications in Japan and the U.S. industry in the early 1980s. It has been found that SAP has the potential to replace fluff, making their use in sanitary products such as baby diapers and sanitary napkins cost-effective.

[0003] The desired characteristics of SAP include high absorption capacity, high and adjustable swelling rate, absorbency under high load, good swelling gel strength, high gel fraction after cross-linking, excellent durability and stability when swelling and during storage, non-toxicity and low cost. Although current hydrogel systems provide good performance in several aspects in these different aspects, there are several disadvantages in various preparations, including low absorbency under pressure, gel blocking (the initial layer of SAP forms a relatively impermeable barrier to subsequent water diffusion and deeper absorption into the material) and high sensitivity to electrolyte solutions. Various strategies have been adopted to address these challenges, including the formation of composite and nanocomposite hydrogels, interpenetrating polymer network (IPN) hydrogels and various surface treatments; However, there is still a need for improvement to enable the use of minimal materials in the widest possible range of applications.

[0004] The nature of the monomers and cross-linking agents, their concentrations and molar ratios are known to be the most important factors affecting the absorption capacity of SAPs. Acrylic acid, acrylamide and methacrylic acid are the most widely used monomers for commercial preparation of SAPs. However, the presence of some residual acrylamide in the gel poses a challenge to the practical use of such hydrogels for human health and personal care products. In contrast, the water absorption and swelling properties of ionic SAPs (e.g. based on acrylic acid or methacrylic acid) are significantly reduced in saline liquids, including physiological fluids such as urine and blood. The reason for this salt sensitivity is that counterions such as sodium ions (Na +) can effectively shield the polymer backbone charge, leading to condensation of counterions with polymer-bound charged groups and thereby reducing the counterion entropy and direct chain-chain repulsion available to drive the swelling response.

[0005] Conventional SAM is mainly made of two types of SAP: synthetic polymers and natural polymers. In general, synthetic superabsorbent polymers are charged polyelectrolytes, such as polyacrylic acid (PAA), polyvinyl sulfonic acid, polyvinyl phosphoric acid salts and partially hydrolyzed maleic anhydride copolymers. Natural polymers include both neutral polymers and charged polymers, such as carboxymethyl cellulose, sodium alginate, chitosan salts and modified starch. All of these known SAMs have substantial limitations. For example, the most widely used SAM based on commercial PAA has limited absorbency under load (AUL) and is also very sensitive to salt.

[0006] The salt sensitivity of SAM leads to a decrease in the gel swelling capacity. In order to compensate for the reduced capacity caused by salt sensitivity, personal care garments require more SAM materials to ensure sufficient absorption capacity to prevent leakage. Therefore, the personal care industry urgently needs to improve or overcome the salt sensitivity of conventional SAM materials.

[0007] However, SAM salt sensitivity is a challenging problem that needs to be solved. Although many attempts have been made in the art, all proposed solutions remain impractical and cost-prohibitive. It is well known in the art that the major part of a SAM is in the form of its neutralized salt, and the conventional thinking is that all these neutralized salt units are considered to be in their fully ionized form, such as metal ions (e.g., Na + ) are free to move during swelling. It is also known in the art that salt is detrimental to capacity, and that high-valent inorganic salts inhibit SAM capacity more than monovalent salts (such as sodium chloride). Therefore, past work on reducing the salt sensitivity of SAM materials has focused on simply using more SAM material to compensate for capacity loss, removing / reducing salt from physiological fluids (such as urine), or attempting to design new structures that are less salt-sensitive.

[0008] In PCT / US2020 / 053003, it is described that copolymerization of SAM monomers with selected inorganic salts having metal ions with an oxidation state of at least 2 can provide significant increases in CRC performance without deleterious effects on other performance attributes (such as AUL). However, these copolymerizations were achieved using non-staged one-pot synthetic procedures. One-pot synthetic procedures are simple to manufacture, but they have the obvious disadvantage of not providing flexibility in controlling / designing the SAM polymer chain structure to mitigate salt sensitivity. For example, uniform crosslinking density throughout the gel network will limit elastic expansion, so that the potential capacity increase caused by chain charge-charge repulsion will be reduced.

[0009] SAMs and methods of making SAMs are described herein. The SAMs are copolymerized with selected redox-active inorganic salts in a staged polymerization process. The copolymer-based SAMs have significantly improved absorption properties due to the increased presence of permeating free ions. The copolymer-based SAMs also have an interpenetrating network due to the staged copolymerization procedure, which can alleviate elastic forces that limit chain expansion. Copolymer-based SAMs also have structural design flexibility, where each stage of the polymerization can have its own composition, crosslink density, etc., which can further increase the absorption capacity of the SAM while providing unique SAM properties that traditional uniform PAA-based SAM structures may not provide.

[0010] Compositions and methods according to the present disclosure can be used in a variety of absorbent products.

[0011] Purpose of the Invention

[0012] The purpose of the present disclosure is to address the salt sensitivity of AA-based SAMs by using a staged polymerization technique. Summary of the invention

[0013] In one aspect, the present invention provides a superabsorbent polymer comprising a polymer backbone, wherein the polymer backbone comprises (i) a neutralized backbone monomer, (ii) a neutralized backbone monomer complexed with a coordination complex, wherein the coordination complex comprises a metal ion in an oxidation state of at least 2, (iii) optionally an unneutralized backbone monomer, and (iv) optionally an unneutralized backbone monomer complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2, and optionally a crosslinker; wherein the superabsorbent polymer comprises a non-uniform microstructure.

[0014] On the other hand, the present invention provides a method for preparing a superabsorbent polymer, the method comprising: (i) an initial polymerization stage, the initial polymerization stage comprising (ia) forming a mixture, the mixture comprising a solvent, a monomer, a salt comprising a redox-active metal ion, an optional crosslinker and an initiator, and (ib) reacting the mixture at a first temperature; and (ii) a final polymerization stage, the final polymerization stage comprising (iia) optionally adding a crosslinker to the mixture; (iib) heating the mixture from the first temperature to a second temperature; and (iic) reacting the mixture at the second temperature.

[0015] In yet another aspect, provided herein is a method of using a superabsorbent polymer comprising a polymer backbone comprising (i) a neutralized backbone monomer, (ii) a neutralized backbone monomer complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2, (iii) an optional unneutralized backbone monomer, and (iv) an optional unneutralized backbone monomer complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2, and an optional crosslinker; wherein the superabsorbent polymer comprises a non-uniform microstructure. The method comprises using the superabsorbent polymer in a consumer product. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Depicted include stable salts such as FeCl 3 The conventional process of the non-staged SAM polymerization process.

[0017] Figure 2 According to an exemplary embodiment of the present disclosure, the figure depicts FeCl 2 Induced staged SAM polymerization.

[0018] Figure 3A According to an exemplary embodiment of the present disclosure, the figure depicts a FeCl 2 Two-dimensional view of the polymer microstructure resulting from the induced staged SAM polymerization.

[0019] Figure 3B According to an exemplary embodiment of the present disclosure, the figure depicts a FeCl 2 Three-dimensional view of the polymer microstructure resulting from the induced staged SAM polymerization.

[0020] Figure 4 is a graph depicting storage modulus data for a polymer produced by staged polymerization and a polymer not produced by staged polymerization, according to an exemplary embodiment of the present disclosure.

[0021] Figure 5 is a graph depicting storage modulus data for polymers produced by staged polymerization, according to an exemplary embodiment of the present disclosure.

[0022] Figure 6 is a graph depicting selected inorganic salts for increasing ionization, according to an exemplary embodiment of the present disclosure.

[0023] Figure 7 is an exemplary embodiment of the present disclosure, the figure depicting a single iron (II) complex prior to polymerization.

[0024] Figure 8is a diagram depicting the coordination patterns of two iron (II) complexes before polymerization, according to an exemplary embodiment of the present disclosure.

[0025] Fig. 9 is a diagram depicting a potential AANa-SIS unit formed from a single iron(II) complex in a polymeric network, according to an exemplary embodiment of the present disclosure.

[0026] Fig.10 is a diagram depicting a potential AANa-SIS unit formed from a bidentate iron(II) monomer complex in a polymeric network, according to an exemplary embodiment of the present disclosure. DETAILED DESCRIPTION

[0027] Superabsorbent polymers produced by copolymerization of SAM monomers with selected inorganic salts having metal ions having an oxidation state of at least 2 are described in PCT / US2020 / 053003, which is incorporated by reference. These copolymerizations are achieved using a non-staged one-pot synthetic procedure. Figure 1 shows that including stable salts such as FeCl 3 An example of a non-staged SAM polymerization process. In the conventional process, a pre-polymerization mixture is prepared at 0°C or room temperature, and a stable metal salt is added to the pre-polymerization mixture. These stable metal salts do not initiate polymerization. Instead, the single-step polymerization occurs via a single-step thermal free radical polymerization, where the temperature is raised to 60°C-70°C and maintained at that temperature to complete the polymerization. This results in an almost uniform polymer structure with uniform crosslink density.

[0028] In contrast to non-staged one-pot synthetic procedures and resulting polymers, the present disclosure relates to SAMs copolymerized with selected redox-active inorganic salts in a staged polymerization process. Figure 2 The staged polymerization process is depicted in FIG. This exemplary staged polymerization process has two stages. Typically, in such a two-stage process, a prepolymer mixture is prepared at a relatively low temperature (such as 0° C. and / or an ice bath) or at room temperature. A crosslinking agent may or may not be added to the prepolymer mixture. A crosslinking agent having a redox active metal (such as FeCl 2) is added to the mixture to initiate the first stage redox induced polymerization while providing ionization enhancement. This produces water-soluble oligomers. In the absence of added crosslinking agents in the prepolymerization mixture, there will be no crosslinking or reduced crosslinking. Crosslinking agents may or may not be added to water-soluble oligomers. Next, a second stage thermal free radical polymerization is initiated by increasing the temperature to 60°C-70°C and maintaining it at that temperature to complete the polymerization. This produces a polymer comprising a shell-core microstructure, wherein the first stage oligomers account for 1%-30% of the final polymer dry weight, and the second stage polymers account for 60%-99% of the final polymer dry weight. After the second stage polymerization, the polymer is water-insoluble.

[0029] The staged polymerization process according to the present disclosure provides a first function of incorporating a small amount of selected inorganic salts (SIS) into a superabsorbent material (SAM) mainly based on PAA for absorption capacity enhancement. Moreover, in addition to the first capacity enhancement function, the staged polymerization process according to the present disclosure provides a second function of controlling the polymerization process, so that the gel properties of the SAM polymer can be further improved. In this second function, the SIS will be part of the polymerization initiation step and must be redox active. In other words, when the SIS reacts with a suitable free radical polymerization initiator (e.g., KPS) to start the polymerization process, they must be able to be oxidized from a lower oxidation state (e.g., M n+ ) is oxidized to a higher oxidation state (e.g. M n+1 By initiating the polymerization process, the oxidized metal ion form (e.g. M n+1 ) will be incorporated into the polymer chain by complexation to provide a source of ionization enhancement. Non-redox active salts can still be added for the purpose of ionization enhancement, but they will not initiate polymerization.

[0030] Control of polymerization means that the secondary function of the redox-active SIS will allow the polymerization process to proceed in pre-designed stages such as stage 1, stage 2, stage 3, etc. Stage 1 is the polymerization initiation step, and its polymerization parameters can be the same or different compared to other stages. The polymerization parameters here include, but are not limited to, temperature, time, oxygen level, crosslinking agent, initiator, one or more monomers, the concentration of each monomer, initiator, crosslinking agent (e.g., loading level), and any specially designed reaction-related sequence (e.g., the order of addition of monomers or initiators or crosslinking agents, etc.). For example, stage 1 may or may not require a crosslinking agent, so that the polymer network formed in this step may be mainly a long-chain polymer without crosslinking based on chemical bonds. In another example, both stage 1 and stage 2 may have a crosslinking agent, but two different temperatures and different polymerization times are required to complete their respective polymerization processes.

[0031] The polymer networks formed by different stages according to the present disclosure are not independent. Instead, the polymer networks formed at different stages are interconnected by chemical crosslinking, physical chain-chain entanglement, or chain charge-charge interaction, etc. In some cases, such interconnection may lead to a hierarchical network structure, while in other cases, the overall structure may be more like an interpenetrating network because some parts of the networks from different stages are effectively entangled together by chemical crosslinking, charge-charge interaction, and physical entanglement.

[0032] In a general embodiment using acrylic acid-based monomers as an example, selected inorganic salts (SIS), including redox-active salts, can be added to acrylic acid (AA) or partially neutralized AA solutions to allow the SIS to form AA-SIS and AANa-SIS complexes prior to polymerization. After complex formation, a conventional polymerization procedure is performed to form the desired sample material. Alternatively, the SIS can be added to the polymerization procedure as the last reagent, and if they are added to the monomers first, this can prevent premature polymerization initiation. In addition, the SIS can be added in batches at each stage or at different stages at the desired ratio. The preferred loading range of SIS can vary, but will generally not exceed 1% of the weight of the monomers involved.

[0033] The general structure of the SAM materials of the present disclosure can be described as a phased overall network, where each phase has its own sub-network:

[0034] [network] 第1阶段 [network] 第2阶段 …[network] 第x阶段 [network] 第x1阶段 …

[0035] Generally, the number of stages can be any suitable number of stages known in the art. The number of stages can be one, two, three, four, five or more than five. Preferably, the total number of stages should be controlled below five, and most preferably controlled below three.

[0036] The network of different stages can be any desired ratio, and can be controlled by changing the polymerization parameters as described above. In some embodiments, one stage will be dominant. In some embodiments, these stages are evenly divided. In some embodiments, the transition from one stage to the next stage is considered to be a separate stage, because the transition can be time-dependent or temperature-dependent or similar. For example, it takes time for the polymerization mixture to transition from one temperature to another temperature, because raising the temperature may require time (e.g., continuous or pre-prepared temperature baths).

[0037] Due to the complexity of precisely defining the exact network structure of each polymerization stage, the present disclosure adopts a simplified approach by using the total loading level of each monomer and the SIS complex form of each monomer to define the composition of the final polymer. For example, if the staged polymerization involves two monomers and a redox SIS salt, the composition of the final polymer can be described as [(monomer 1) x (Monomer 1-SIS) y (Single 2) z (Monomer 2-SIS) w ], where x, y, z, w are the molar or weight ratios of each component. In terms of weight ratio, the combined Y and W ratio is generally limited to less than 1% of (x+y+z+w). In a specific example, for two monomers of acrylic acid and sodium salt of acrylic acid, the composition of the staged copolymer can be described as [(AA) x (AA-SIS) y (AANa) z (AANa-SIS) w ], where x, y, z, w are the molar ratio or weight ratio of each monomer and their SIS complex form.

[0038] In many embodiments, a superabsorbent polymer according to the present disclosure comprises a polymer backbone comprising (i) a neutralized backbone monomer, (ii) a neutralized backbone monomer complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2, (iii) optionally an unneutralized backbone monomer, and (iv) optionally an unneutralized backbone monomer complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2, and optionally a crosslinker, wherein the superabsorbent polymer comprises a non-uniform microstructure.

[0039] In some embodiments, the superabsorbent polymer comprises a plurality of polymer fractions, wherein each polymer fraction is produced in a different polymerization stage. In some embodiments, the superabsorbent polymer comprises a first polymer fraction and a second polymer fraction, wherein the first polymer fraction and the second polymer fraction are produced in different polymerization stages.

[0040] In some embodiments, the superabsorbent polymer comprises a first polymer fraction present in an amount in the range of about 1 to about 40 weight percent of the superabsorbent polymer and a second polymer fraction present in an amount in the range of about 60 to about 99 weight percent of the superabsorbent polymer. In some embodiments, the superabsorbent polymer comprises a first polymer fraction present in an amount in the range of about 1 to about 30 weight percent of the superabsorbent polymer and a second polymer fraction present in an amount in the range of about 60 to about 99 weight percent of the superabsorbent polymer.

[0041] Typically, the superabsorbent polymer may comprise any suitable non-uniform microstructure known in the art. The non-uniform microstructure results in a non-uniform polymer structure. In some embodiments, the superabsorbent polymer comprises a non-uniform microstructure selected from the group consisting of: a layered polymer structure with domains from different stages, a core-shell polymer structure comprising a core from one stage and a shell from another stage, an interpenetrating network with one stage as one network and another stage as another network, and combinations thereof.

[0042] exist Figure 3A 2D view and Figure 3B An exemplary core-shell polymer microstructure is shown in the three-dimensional view in FIG.

[0043] In general, the superabsorbent polymer may have any suitable crosslink density known in the art. In some embodiments, the superabsorbent polymer has a non-uniform crosslink density. In some embodiments, the superabsorbent polymer comprises a first polymer portion having a first crosslink density and a second polymer portion having a second crosslink density, wherein the first crosslink density and the second crosslink density are different. In some embodiments, the superabsorbent polymer comprises a first polymer portion having no crosslinks or minimal crosslinks and a second polymer portion having a high degree of crosslinks.

[0044] Typically, superabsorbent polymers have unique absorption properties compared to conventional superabsorbent polymers. In some embodiments, the superabsorbent polymer is configured to provide at least 5.2% storage modulus (G') reduction between 300 seconds and 500 seconds after exposure to a 0.9% NaCl solution at room temperature. In contrast, under the same test conditions, polymers that are not produced by staged polymerization will not show such a large storage modulus (G') reduction.

[0045] Typically, superabsorbent polymers are copolymerized from selected inorganic salts, neutralized monomers, unneutralized monomers, and optionally crosslinking agents. Such copolymerized superabsorbent polymers reduce salt sensitivity to significantly improve CRC performance without adversely affecting other performance attributes such as AUL. Higher AUL can also be achieved if the gel strength of the SAM according to the present disclosure can be enhanced using well-known techniques such as surface crosslinking of the SAM particles.

[0046] The metal ion with an oxidation state of at least 2 can have an oxidation state of at least 2, at least 3 or at least 4. The use of a stable selected inorganic salt comprising such a metal ion is based on a key discovery in the analysis of the interaction of metal salts with SAM polymer chain ion pairs. When a metal salt, especially a metal salt with an oxidation state of the metal ion greater than two in the salt, interacts with the polymer chain of the SAM from an external solution, and when the same salt is introduced into the polymer chain by forming a metal complex with a monomer before polymerization, there is a major difference. In the former case, the salt approaches the ion pair of the polymer chain as an "external" ion, and they mainly act as a chain charge shielding agent (a single counter ion (such as Na + ) and high oxidizing ions (such as Ca 2+ and Al 3 + )) and chelating crosslinkers (highly oxidizing ions (such as Ca 2+ 、Al 3+ The shielding and chelation of highly oxidized metal ions is deeper because they will accumulate on the outer layer of the SAM particles, so that the elastic part of the SAM swelling will be significantly restricted and reduced. However, for the latter case, the same highly oxidized metal ions, when they first form a complex with a monomer such as AA or AANa and then polymerize, can actually help to generate more free ions for the polymer chain, thereby increasing the SAM absorbency, such as Figure 6 This observation is consistent with the osmotic pressure theory, which states that the osmotic pressure is proportional to the total particle count in the gel system.

[0047] These complex salts are referred to as "internal" or "intrinsic" metal salts and metal ions.

[0048] However, even if the SAM absorbency can be increased, too much inner salt can still be harmful to the SAM absorbency because they can also act as cross-linking agents through chelation. Therefore, only when the chelation between polymer chains during polymerization is minimized, the absorption benefit can be achieved and the SAM capacity is effectively improved. For this reason, the loading level of the metal salt used to form the complex must be managed so that ionization can be maximized and cross-linking can be minimized. In addition, only selected salts with metals having an oxidation state greater than two can be suitable as stable selected inorganic salts in the present disclosure. This is because high oxidation state salts are more conducive to forming more free ions than salts with low oxidation state metal ions. More specifically, metal ions (i.e., M2) with an oxidation state of two can be used as stable inorganic salts. 2+ ) than the metal ion with oxidation state 1 (i.e. M + ) is more favorable in a stable selected inorganic salt, and the oxidation state is tri or greater metal ions (i.e., M ≥3+ ) than the metal ion in oxidation state II (i.e. M 2+ ) is more advantageous.

[0049] Since few metal ions are stable when the oxidation state is greater than three, the preferred salts are those with metal ions in an oxidation state of at least three. 3+ Salts of the compounds may still not be suitable for use in the present disclosure if they tend to form chelate structures in aqueous solutions or polymeric mixtures.

[0050] Many inorganic salts have metal ions (i.e., metal halides, metal sulfates, and metal nitrates) with an oxidation state greater than 2, which can be used to demonstrate the beneficial effects of the present disclosure. However, most of these salts are not easily available and have safety issues in personal care applications. Therefore, the stable metal ions shown herein are common in nature and are related to biologically relevant processes. Therefore, they are safe or considered safe in at least some personal care applications. In any case, it is not intended to limit the present disclosure, and any inorganic salt with a metal ion with an oxidation state of at least two can be used as a stable selected inorganic salt in the present disclosure.

[0051] The stable selected inorganic salts according to the present disclosure include metal ions that can form coordination complexes with the monomers in the prepolymerization mixture; these structures will become part of the polymer chain or chain network of the SAM after copolymerization. The stable selected inorganic salts are non-redox active salts that contribute to ionization enhancement but do not initiate polymerization.

[0052] The structure of a coordination complex depends in part on the coordination number of the metal ion. The coordination number of a metal is largely determined by how many donor atoms can fit around the metal, which in turn is controlled by size. With respect to transition metals, late transition metals are smaller than early transition metals. When crossing the 3d transition series, the nuclear charge and atomic number increase, but the shielding due to filled electron shells remains the same. This pulls the outer electrons closer together, so the atoms and ions become progressively smaller. For zinc, the last and smallest of the 3d metals, four is the most common coordination number. Therefore, late transition metals generally form smaller complexes than early transition metals.

[0053] In some embodiments, the coordination complex comprising a metal ion having an oxidation state of at least 2 is coordinated with more than one neutralized or unneutralized backbone monomer. It is contemplated that monomer complexes having more than one neutralized or unneutralized backbone monomer or combinations thereof can initiate one or two or more polymer chains. Due to these geometrical restrictions of the coordinated metal center ion, a SAM material having such a structure will result in more favorable gel properties, such as improved gel rigidity and mechanical properties.

[0054] like Figures 7 to 10As depicted, the coordination mode between the monomer and the selected salt can have two main modes, for example, one is the coordination between the olefin double bond of the monomer and the metal center, and the other is the coordination between the carboxylate side of the monomer and the metal center. Compared with the olefin double bond coordination, the coordination between the carboxylate and the metal center is more complicated because it can present different modes. It is conceivable that this different coordination mode can be formed before the polymerization of the monomer complex stage, and some of these initial simple complexes can form more complex structures during the polymerization process or even later (such as during the drying process). It is also conceivable that this different interaction can occur within a single polymer chain or between different chains to form a network. For the purpose of ionization enhancement, the network formed by different chains here is not desired and should be minimized because it will act as a cross-linking agent for eliminating ionization.

[0055] Because different coordination modes and the formation of different selected metal salts can make one or more modes superior to other modes, it should be understood here that those skilled in the art can fine-tune the polymerization and processing conditions for a given selected salt so that the maximum capacity enhancement can be achieved. It is also conceivable that in some cases, the CRC enhancement can be deeper than the AUL enhancement, such as the polymerization conditions disclosed herein. In other cases, the AUL enhancement can be deeper than the CRC increase. In other other cases, both the CRC and AUL increases can be achieved.

[0056] Transition metals are particularly advantageous in the present disclosure because they have many oxidation states and coordination complexes. In some embodiments, the coordination complex comprises a metal ion selected from the group consisting of transition metals. Preferably, the coordination complex comprises a metal ion selected from the group consisting of row 1 and row 2 transition metals. Most preferably, the transition metal ion is selected from the group consisting of row 1 transition metals and combinations thereof.

[0057] In some embodiments, the coordination complex comprises a metal ion selected from the group consisting of: Ca 2+ 、Co 2+ 、Zn 2+ , Mn 2+ 、Al 3+ , Fe 3+ 、Co 3+ , Mn 3+ And combinations thereof. In some embodiments, the coordination complex comprises a complex selected from the group consisting of: ML x 2+ ML x 3+ And combinations thereof, wherein L is an organic ligand, and M is a metal ion selected from the group consisting of: Ca 2+ 、Co2+ 、Zn 2+ , Mn 2+ 、Al 3+ , Fe 3+ 、Co 3+ , Mn 3+ 、Ru 3+以 and their combinations.

[0058] The coordination of an organic ligand to a metal center can significantly alter the oxidation potential of the metal center, thereby allowing the polymerization conditions to be altered to accommodate a more redox-sensitive metal center. The use of organic ligands can be particularly helpful in stabilizing some very unstable metal salts, such as Co 3+ and Mn 3+ , so that they can be like Fe 3+ Suitable organic ligands (eg, L) may include, but are not limited to, monodentate, bidentate, and polydentate ligands, such as those commonly used in inorganic / organic / organometallic chemistry. Specific examples include OR 2 NR 3 , PR 3 , OR 2 (CH 2 ) n OR 2、 NR 2 (CH 2 ) n NR 2 , PR 2 (CH 2 ) n PR 2 etc., wherein R is an alkyl group selected from the group consisting of methyl, ethyl, butyl, and combinations thereof.

[0059] In some embodiments, the coordination complex comprising a metal ion having an oxidation state of at least 2 is coordinated to more than one neutralized or unneutralized backbone monomer. The coordination to more than one neutralized or unneutralized backbone monomer can occur along the same or different polymer chains.

[0060] Non-redox active stable selected inorganic salts may also be added for the purpose of ionization enhancement, but they do not initiate polymerization. A particularly preferred stable selected inorganic salt is FeCl 3 .FeCl 3 It is particularly effective and inexpensive. FeCl 3 It exists in the form of a variety of hydrated coordination complexes in water. The hydrated forms can form monodentate complexes, bidentate complexes, and even higher multidentate complexes from monomers, and they can be retained and become the source of more free ions in the polymerized SAM unit ( Figures 7 to 10As depicted and described herein, selected inorganic salts can improve the salt sensitivity of a SAM by a number of mechanisms, primarily by increasing the free ions when they are incorporated directly into the polymer chains and chain networks of the SAM as intrinsic internal salts.

[0061] Although not specifically directed to, compared with the SAM without coordinated metal ions, the SAM with metal ions may have other favorable properties. For example, the charged metal center is known for capturing or killing bacteria, and this property is extremely desirable for personal clothing (such as diapers and pants and feminine pads). In another aspect, known metal ions can also absorb various odor molecules, such as ammonia, amines and sulfur compounds. It is well known that these odor compounds are present in physiological fluids (such as urine, blood, sweat, etc.). In another aspect of the present disclosure, the metal ions in polymer chains and chain networks can serve as the starting point of degradation, so that they can decompose faster in nature or engineering processes, thereby accelerating the decomposition process such as by light radiation (such as commonly referred to as OXO-biodegradation process). Therefore, the SAM with coordinated metal ions may be superior to other SAMs, at least because they have better biodegradability.

[0062] Typically, the neutralized backbone monomers are present in an amount in the range of about 50 to about 99 mole % of the superabsorbent polymer, the neutralized backbone monomers complexed with the coordination complex comprising the metal ion in an oxidation state of at least 2 are present in an amount in the range of about 0.001 to about 0.3 mole % of the superabsorbent polymer, the unneutralized backbone monomers are present in an amount in the range of about 0 to about 40 mole % of the superabsorbent polymer, and the unneutralized backbone monomers complexed with the coordination complex comprising the metal ion in an oxidation state of at least 2 are present in an amount in the range of about 0.001 to about 0.3 mole % of the superabsorbent polymer. More neutralized backbone monomers complexed with the coordination complex comprising the metal ion in an oxidation state of at least 2 can have a deleterious effect on the superabsorbent polymer. In some embodiments, the preferred total amount of neutralized and unneutralized monomers with a coordinated selected salt is in the range of about 0.01 mole % to about 0.3 mole % of the final polymer.

[0063] In some other embodiments, the preferred total amount of neutralized and unneutralized monomers with coordinated selected salts is in the range of about 0.01 mol % to about 0.15 mol % of the final polymer. In some other embodiments, the preferred total amount of neutralized and unneutralized monomers with coordinated selected salts is in the range of about 0.01 mol % to about 0.1 mol % of the final polymer. In some other embodiments, the preferred total amount of neutralized and unneutralized monomers with coordinated selected salts is in the range of about 0.01 mol % to about 0.05 mol % of the final polymer.

[0064] In some embodiments, the neutralized backbone monomer is present in an amount greater than about 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, 85 mol%, 90 mol%, 95 mol%, 96 mol%, 97 mol% or 98 mol% of the superabsorbent polymer.

[0065] In some embodiments, the unneutralized backbone monomer is present in an amount greater than about 0 mol%, 5 mol%, 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 36 mol%, 37 mol%, 38 mol% or 39 mol% of the superabsorbent polymer.

[0066] In some embodiments, the sum of the weight % of neutralized backbone monomers complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2 and the weight % of unneutralized backbone monomers complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2 is less than about 0.2%, less than about 0.075%, less than about 0.050%, less than about 0.025%, and less than 0.01% of the total weight % of the polymer backbone.

[0067] Depending on the final application, superabsorbent polymers can take a variety of forms. In some embodiments, the superabsorbent polymer is in the form of a group selected from the following: particles, gels, fibers, beads, liquids, solids, pastes or combinations thereof. In some specific embodiments, the superabsorbent polymer is a gel or a particle, and is preferably in the form of a particle.

[0068] In some embodiments, the superabsorbent polymer is in the form of a diameter ranging from about 100 μm to about 1000 μm, from about 100 μm to about 900 μm, from about 100 μm to about 800 μm, from about 100 μm to about 700 μm, from about 100 μm to about 600 μm, from about 100 μm to about 500 μm, from about 100 μm to about 400 μm, from about 100 μm to about 300 μm, or from about 100 μm to about 200 μm. In some embodiments, the superabsorbent polymer is in the form of a diameter ranging from about 200 μm to about 900 μm, from about 300 μm to about 800 μm, from about 300 μm to 600 μm, from about 400 μm to about 700 μm, or from about 500 μm to about 600 μm.

[0069] In some specific embodiments, the superabsorbent polymer is in the form of a particle having a diameter ranging from about 300 μm to about 600 μm.

[0070] In various embodiments, the superabsorbent polymer exhibits substantially improved absorbency and salt sensitivity properties without crosslinking. However, crosslinking agents can be used to further enhance the properties of the superabsorbent polymer. The superabsorbent polymer can contain one, two or more crosslinking agents.

[0071] In some embodiments, the superabsorbent polymer comprises a crosslinker selected from the group consisting of methylene (bis)acrylamide (MBAA), poly(ethylene glycol diacrylate) (PEGDA), ethylene glycol diacrylate (EGDA), ethylene glycol dimethacrylate (EGDMA), poly(ethylene glycol dimethacrylate) (PEGDMA), and combinations thereof.

[0072] In some embodiments, the superabsorbent polymer comprises a slightly crosslinked polymer portion. In some embodiments, the superabsorbent polymer comprises a polymer portion having a crosslinker density in the range of about 0.1 mol % to about 2.0 mol %. In some embodiments, the superabsorbent polymer comprises a polymer portion having a crosslinker density in the range of about 0.2 mol % to about 2.0 mol %. In some embodiments, the superabsorbent polymer comprises a polymer portion having a crosslinker density in the range of about 0.5 mol % to about 2.0 mol %. In some embodiments, the superabsorbent polymer comprises a polymer portion having a crosslinker density in the range of about 1.0 mol % to about 2.0 mol %. In some embodiments, the superabsorbent polymer comprises a polymer portion having a crosslinker density in the range of about 1.5 mol % to about 2.0 mol %.

[0073] The neutralized backbone monomer and the unneutralized backbone monomer are each selected individually according to the final application of the superabsorbent polymer. Monomers known in the art for superabsorbent polymers are suitable as neutralized backbone monomers and unneutralized backbone monomers. The neutralized backbone monomer and the unneutralized backbone monomer can be the neutralized and unneutralized forms of the same monomer or the neutralized and unneutralized forms of different monomers.

[0074] In some embodiments, the neutralized backbone monomer and the unneutralized backbone monomer are each individually selected from the group consisting of acrylic acid, methacrylic acid, vinyl sulfonic acid, vinyl phosphoric acid, partially hydrolyzed maleic anhydride, and combinations thereof.

[0075] Also disclosed herein is a method for preparing a superabsorbent polymer, the method comprising: (i) an initial polymerization stage, the initial polymerization stage comprising (ia) forming a mixture comprising a solvent, a monomer, a salt comprising a redox-active metal ion, an optional crosslinker and an initiator, and (ib) reacting the mixture at a first temperature; and (ii) a final polymerization stage, the final polymerization stage comprising (iia) optionally adding a crosslinker to the mixture; (iib) heating the mixture from the first temperature to a second temperature; and (iic) reacting the mixture at the second temperature.

[0076] The salt containing the redox-active metal ion is part of the polymerization initiation step. When reacting with a suitable free radical polymerization initiator (e.g., KPS) to start the polymerization process, the redox-active metal must be able to convert from a lower oxidation state (e.g., M n+ ) is oxidized to a higher oxidation state (e.g. M n+1 By initiating the polymerization process, the oxidized metal ion form (e.g. M n+1 ) will be incorporated into the polymer chain by complexation to provide a source of ionization enhancement. Non-redox active salts can still be added for the purpose of ionization enhancement, but they will not initiate polymerization.

[0077] In some embodiments, the salt comprising a redox-active metal ion comprises a metal ion selected from the group consisting of: Co 2+ , Mn 2+ 、Al 2+ , Fe 2+ 、Co 2+ , Mn 3+ 、Ru 2+ And combinations thereof. Generally, the salt may comprise any suitable salt anion known in the art. In some embodiments, the salt comprises an anion selected from the group consisting of: Cl - 、SO 4 2- 、NO 3 - , BF 4 - , and combinations thereof.

[0078] A particularly preferred redox-active metal salt is FeCl 2 .FeCl 2 is particularly effective and inexpensive. During polymerization, Fe 2+ Oxidized to Fe 3+ .

[0079] In some embodiments, the redox-active metal ion is oxidized to an oxidized metal ion selected from the group consisting of: Co 3+ 、Al 3+ , Fe 3+ 、Co 3+ , Mn 3+ and their combinations.

[0080] In some embodiments, the mixture further comprises a stable salt comprising a metal ion in an oxidation state of at least 2.

[0081] In some embodiments, the method also includes at least one intermediate polymerization stage between the initial polymerization stage and the final polymerization stage. At least one intermediate polymerization stage may include any suitable conditions for inducing polymerization. In some embodiments, at least one intermediate polymerization stage includes adding a crosslinking agent to the mixture. In some embodiments, at least one intermediate polymerization stage includes a time-dependent transition or a temperature-dependent transition. As used herein, time-dependent transition means the time period of inducing different polymerization stages, such as a time delay. As used herein, temperature-dependent transition means the temperature of inducing different polymerization stages.

[0082] Typically, the method may include any suitable number of polymerization stages known in the art. In some embodiments, the method includes one, two, three, four, five or more than five polymerization stages. In some embodiments, the method includes a plurality of polymerization stages in the range of 2 to 5.

[0083] Typically, the first temperature can be any temperature that promotes the reaction. In some embodiments, the first temperature is in the range of about -20°C to about 40°C. In some preferred embodiments, the first temperature is 0°C. In some preferred embodiments, the first temperature is in the range of about 20 to about 25°C.

[0084] Typically, the second temperature can be any temperature that promotes the reaction. In some embodiments, the second temperature is in the range of about 20°C to about 100°C. In some embodiments, the second temperature is in the range of about 40°C to about 70°C. In some preferred embodiments, the second temperature is in the range of about 60°C to about 70°C.

[0085] The method steps of initiating the reaction can be implemented using standard materials and procedures known in the art, including adding an initiator, a accelerator, or a combination thereof to the mixture. In some specific embodiments, the initiator is an oxidizing agent.

[0086] The initiator can be an organic compound. In some embodiments, the initiator is selected from the group consisting of an azo compound, an organic peroxide compound, an organic persulfate compound, and combinations thereof.

[0087] The initiator can be an inorganic compound. In some embodiments, the initiator is selected from the group consisting of inorganic peroxide compounds. In some specific embodiments, the initiator is selected from the group consisting of potassium persulfate, ammonium persulfate, and combinations thereof.

[0088] Some reactions can be carried out at a suitable rate in the absence of a promoter. When a promoter is used, the promoter is an organic compound. In some embodiments, the promoter is selected from the group consisting of an organic compound, an organic base, tetramethylethylenediamine (TEMED), sodium pyrosulfite (SPS), no promoter, and combinations thereof.

[0089] An inert atmosphere improves the reaction by limiting air oxidation. An inert atmosphere can be static or dynamic. When the inert atmosphere is dynamic, an inert gas continuously flows through the reactants. An inert atmosphere includes a chemically inert gas. In some embodiments, the inert atmosphere is selected from the group consisting of: N 2 , CO 2 , noble gases, helium, neon, argon, krypton, xenon and combinations thereof. In some specific embodiments, the method step of reacting the mixture comprises reacting the mixture under N 2 react in an inert atmosphere.

[0090] In some embodiments, the method further comprises drying the reaction product. The reaction product can be dried in an oven or by other known drying means. The drying temperature and time can vary according to the relative moisture content and properties of the reaction product. In some embodiments, the method further comprises drying the reaction product at a temperature in the range of about 50 ° C to about 100 ° C. In some specific embodiments, the method further comprises drying the reaction product at a temperature in the range of about 70 ° C to about 90 ° C.

[0091] In some embodiments, the method further comprises grinding the reaction product. Grinding the reaction product is to grind the reaction product into a desired particle size. Suitable methods are known in the art. In some embodiments, the method further comprises grinding the reaction product with a grinding device selected from the group consisting of a mechanical stirrer, a coffee grinder, a crusher, a pulverizer, a grinder, a mill, and a combination thereof.

[0092] In another aspect of the present disclosure, the particles as described in the present disclosure can be further processed according to well-known procedures (such as particle surface crosslinking). Appropriately selected surface crosslinking agents can enhance the mechanical strength of the particles and help control the intake rate, improve gel permeability and fluid distribution between particles and within a given particle.

[0093] Regarding the properties of the final superabsorbent polymer, the ability of the polymer to absorb fluid under a static load can be measured as Absorbency Under Load (AUL). A typical AUL test format can be used. The ability of a pre-swollen polymer to retain water under a force can be measured as Centrifuge Retention Capacity (CRC). A typical CRC test format can be used.

[0094] Consumer products or superabsorbent materials may comprise superabsorbent polymers according to the present disclosure.Superabsorbent polymers may also be used in consumer products or superabsorbent materials.

[0095] Suitable consumer products include, but are not limited to, personal hygiene products, wipes, napkins, bibs, disposable bed pads, wound dressings, food packaging, infant and adult diaper products, children's training pants, feminine pads and napkins, armbands, agricultural and pet products containing superabsorbent components, disposable absorbent products, and combinations thereof.

[0096] Example

[0097] Without further elaboration, it is believed that one skilled in the art using the preceding description can utilize the present invention to its fullest extent.Therefore, the following examples are to be construed as illustrative only, and not limiting of the present disclosure in any way.

[0098] Measurement technology.

[0099] The polymers according to the present disclosure and examples were measured to determine their absorbency under load (AUL) and centrifuge retention capacity (CRC) properties.

[0100] Technique 1. AUL measurement of SAM particles.

[0101] AUL measures the ability of a polymer to absorb fluid under static load and can be considered a measure of gel swelling combined with gel strength. A typical AUL test format is used, which consists of a simple cylindrical device with a macroporous sintered filter plate at one end of a sintered plastic cylinder. For the sample tested, 160 mg (W 1 ) dried SAP sample and evenly placed on the surface of a polyester gauze, which is placed on top of the sintered plastic. The desired load (e.g., a weight that can produce a pressure of 0.3-0.9 PSI) is then placed on top of the dried SAP particles, where the load is designed to allow it to move freely in the plastic cylinder. The device is placed in a petri dish of 0.9% saline solution on top of the screen (to ensure that water can access the bottom of the sintered plastic) for 1-72 hours or any desired measurement time. The swollen sample (W 2 ), and use Equation 1 to calculate AUL:

[0102]

[0103] Technique 2. CRC measurement of SAM particles.

[0104] In contrast to the AUL test, in which a dry powder of SAP is hydrated under load, the CRC test measures the ability of a pre-swollen SAP to retain water under force. 1) Dry SAP samples were weighed into pre-weighed tea bags. The tea bags were immersed in a 0.9 wt % saline solution for 1-2 hours or any desired length of testing time to swell the SAP. Subsequently, the tea bags were placed in a cylindrical centrifuge tube with a porous interior to allow drainage and centrifuged at 1600 rpm for 3 minutes. As a control, an empty tea bag was also placed in saline and centrifuged at the same speed. After centrifugation, the tea bags were weighed again (W 2 ), and calculate the difference between the dry sample and the swollen sample. The CRC amount is calculated by equation 2:

[0105]

[0106] SAM is copolymerized with a selected stabilizing inorganic salt.

[0107] The following examples are used to demonstrate non-staged copolymerization methods for preparing SAMs copolymerized with selected inorganic salts. These methods and resulting polymers are known in the art, for example in PCT / US2020 / 053003, which is incorporated herein by reference.

[0108] Selected stable inorganic salts (e.g., various inorganic salts including metal ions in an oxidation state of at least 2) are copolymerized with sodium acrylic acid salts (e.g., a major component of the base monomers currently used in commercial SAMs). Samples synthesized without these salts under the same polymerization conditions were used as controls.

[0109] Comparative Example 1. Preparation of PAA-based SAM particles without using metal ions with an oxidation state of at least 2.

[0110] 15 grams of acrylic acid (AA) monomer is added to a glass reaction flask (e.g., a 120 mL wide-mouth round jar, beaker, or round-bottom flask) with a magnetic stirring bar. The glass reaction flask should be equipped with a sealing lid or a glass or rubber stopper. About 45 mL of deionized (DI) water is added to the glass reaction flask with the AA monomer, and then cooled to about 0° C. with an ice-water bath. After cooling, 5.84 g of NaOH flakes with a purity greater than 97% are added to the cold solution. The mixture is then stirred with a magnetic stirrer until the NaOH flakes are completely dissolved. Dissolution under stirring usually takes about 10-20 minutes. Alternatively, neutralization can be performed by adding a pre-prepared NaOH aqueous solution dropwise to the AA / water mixture, with the same final total water volume.

[0111] The mixture is rigorously degassed with high purity nitrogen or argon to remove residual air in the reaction mixture and replace the air in the glass reaction flask. The recommended degassing time is at least 5-10 minutes. About 5 minutes after entering the degassing step, the initiator (about 45 mg 99.99% potassium persulfate (KPS)) and the crosslinking agent (about 68 mg greater than 99% MBAA (N,N-methylenebis(acrylamide))) (both of which were pre-dissolved in 4 mL deionized water at room temperature) are added to the cooled neutralized AA solution dissolved in deionized water. The degassing process is then continued.

[0112] The glass reaction flask is then sealed and transferred to a preheated water bath equipped with a magnetic stirrer to start the single-step thermal free radical polymerization process. The polymerization temperature is controlled in the range of about 60° C. to about 70° C., more specifically about 65° C. The flask is placed directly into the preheated bath, or into a temperature bath starting from room temperature and gradually raised to about 65° C. or any desired final polymerization temperature.

[0113] The gelation time is monitored (e.g., by determining when the magnetic stir bar stops stirring). Gelation of the control sample is observed only when the temperature reaches above 50°C-65°C for at least 5-20 minutes (e.g., the solution becomes viscous and then the stir bar stops stirring). After gelation, the gel is retained in the heating bath for an additional 4 hours to ensure that polymerization is complete.

[0114] After polymerization, the gel is removed from the glass reaction flask. Cut the large gel block into small pieces with a knife or scissors for drying. A stirrer can be used to break the large gel block into small pieces. After cutting, the resulting gel block is dried in an 85°C oven for at least 24-48 hours. Drying can also be accomplished by accelerating the drying process, using an air dryer, using the desired oven temperature, using a hot air stream, and combinations thereof. The drying process can also be performed by a dynamic belt system in combination with heating, vacuum, and through air drying techniques.

[0115] The dried gel mass is then placed in a coffee blender or any suitable tool to break into the desired particle size. A U.S. Standard sieve is used to collect particles having a desired size range (e.g., 300-600 microns).

[0116] Comparative Example 2. Preparation of PAA-based SAM particles using metal ions with an oxidation state of at least 2.

[0117] The reaction procedure of Comparative Example 1 was followed except that after the degassing step, the desired amount of the selected metal salt was added to the mixture, and degassing was continued for an additional 5-10 minutes.

[0118] Staged polymerization of SAMs copolymerized with selected inorganic salts.

[0119] The following examples serve to demonstrate the feasibility of staged polymerization for preparing SAMs copolymerized with selected inorganic salts.

[0120] Example 1. Staged polymerization using iron (II) chloride.

[0121] Two-stage polymerization was carried out with two monomers AA (30%) and AANA (70%), MBAA as a crosslinker and KPS as a free radical polymerization initiator. Selected and redox-active inorganic salts FeCl 2 The first stage copolymerization was initiated at an ice bath temperature of about 0°C to form the first stage network. After the desired reaction time of the first stage, the temperature was raised to 65°C to complete the copolymerization by conventional free radical polymerization to form the second stage network. Table 1 summarizes the results of the polymerization reactions from different FeCl 2 The capacity data of the loading level clearly show that a small amount of FeCl 2 can lead to significant capacity increase, especially for CRC. However, Table 1 also shows that excessive FeCl 2 is undesirable as it may lead to a decrease in capacity. This is because the excess redox FeCl 2 The polymerization can be quenched by direct reaction (e.g., consumption) with the initiator to form a stable oxidized iron(III) salt. 2 The complete quenching of the polymerization was confirmed as no polymerization was observed when the loading level exceeded 30-40 mg.

[0122] Based on these data, FeCl 2 The desired amount of FeCl is between 0.000066 and 0.1 wt % of the Stage 1 mixture, with the best CRC increase observed at about 0.083 wt % of the Stage 1 mixture. 2 The preferred amount is between 0.05 and 0.1 wt % of the stage 1 mixture.

[0123] Table 1. Capacity data for staged polymerization using iron(II) chloride.

[0124]

[0125] Example 2. Varying the time of addition of the crosslinking agent during staged polymerization.

[0126] Three-stage polymerization was carried out with two monomers AA (30%) and AANA (70%) using KPS as a free radical polymerization initiator. MBAA was added as a crosslinker at different times to form the first, second, and third stage networks. Selected redox-active inorganic salts FeCl 2The first stage copolymerization was initiated at an ice bath temperature of about 0°C to form a first stage network, and then the second stage network was formed by adding the crosslinker MBAA at the desired time. After the desired reaction time of the second stage, the temperature was raised to 65°C to complete the copolymerization by conventional free radical polymerization to form the third stage network. Table 2 clearly shows that changing the addition time of the crosslinker can potentially lead to higher capacity SAM materials.

[0127] Table 2. Effect of crosslinker addition time on SAM capacity during staged polymerization.

[0128]

[0129] Example 3. Varying the amount and addition time of the crosslinker during staged polymerization.

[0130] Three-stage polymerization was carried out with two monomers AA (30%) and AANA (70%) using KPS as a free radical polymerization initiator. MBAA was added as a crosslinker at different times and in different ratios to form the first-stage and second-stage networks. The selected redox-active inorganic salt FeCl 2 The first stage copolymerization was initiated at an ice bath temperature of about 0°C to form the first stage network, and then the crosslinker MBAA was added at the desired time and loading level to form the second stage network. After the desired reaction time for the second stage, the temperature was raised to 65°C to complete the copolymerization by conventional free radical polymerization to form the third stage network. Table 3 clearly shows that varying both the amount and addition time of the crosslinker MBAA can potentially lead to higher capacity materials.

[0131] Table 3. Effect of crosslinker addition time on SAM capacity during staged polymerization.

[0132]

[0133] Example 4. Control achieved through a staged polymerization process.

[0134] By precisely controlling the polymerization time of each stage, staged polymerization can be used to control the structure of each stage and its total mass percentage in the final polymer. 2 and KPS were used to initiate copolymerization of acrylic acid (about 30%) and sodium acrylate (about 70%) at an ice bath temperature of about 0°C to form a stage 1 network, and then the polymerization was quenched by pouring the reaction mixture into methanol at the desired polymerization time. The precipitated polymer solids were then collected and dried to quantify the mass percentage of stage 1 in the final polymer. The dried samples were found to be soluble in water, indicating that they mainly constitute the properties of non-crosslinked long-chain polymers. The solubility properties are shown in Table 4.

[0135] Table 4. Time dependence of the 1st stage polymerization without addition of the crosslinker MBAA during the staged polymerization.

[0136]

[0137] The polymer property parameters, including molecular weight (weight fraction Mw, chain number fraction Mn, Z fraction Mz), polydispersity (Mw / Mn), hydrodynamic radius (Rh), intrinsic viscosity (IV) and MKα, were determined and listed in Table 5. Table 5 clearly shows that longer reaction times lead to longer polymer chains, which should be expected to have higher capacity, especially for CRC, due to the low restriction of traditional cross-linking. The data in Tables 4 and 5 support and confirm each other.

[0138] Table 5. Stage 1 polymer property parameters.

[0139]

[0140] Example 5. Polymerization with three monomers with delayed addition of the crosslinker MBAA.

[0141] The three monomers AA (30%), AANA (70%) and VSO 3 Na(vinyl sulfonate sodium salt) was polymerized in two stages with MBAA as crosslinker and KPS as free radical polymerization initiator. Selected and redox-active inorganic salts FeCl 2 The first stage copolymerization was initiated without the use of a crosslinking agent MBAA at an ice bath temperature of about 0°C to form a first stage network. After the desired reaction time of 10 minutes, a crosslinking agent was added to the polymerization mixture, and then the temperature was raised to 65°C to complete the copolymerization by conventional free radical polymerization to form a second stage network. The results are shown in Table 6.

[0142] Table 6. Polymerization with three monomers with delayed addition of the crosslinker MBAA (10 minutes after the start of polymerization).

[0143]

[0144] Comparative Example 3. Staged polymerization using non-redox SIS.

[0145] Non-redox SIS cannot induce a staged polymerization process. Non-redox active salt CaCl 2 、Al 2 (SO 4 ) 3 and FeCl 3 With the redox active salt FeCl 2The same procedure was followed by addition to the polymerization mixture at an ice bath temperature of about 0 °C. 2 No matter how long the reaction mixture was kept and stirred at this temperature, no polymerization was observed. Only when the temperature was raised to conventional thermal free radical polymerization temperatures, e.g., above 50°C-65°C, did polymerization occur, which resulted in a final polymer with a uniform structure.

[0146] Comparative Example 4. Staged polymerization without using selected inorganic salt (SIS).

[0147] A staged polymerization was performed with a control sample without the addition of SIS. The polymerization mixture was prepared with two monomers AA (30%) and AANA (70%) with MBAA as a crosslinker and KPS as a free radical polymerization initiator at an ice bath temperature of about 0°C. No matter how long the reaction mixture was kept and stirred at this temperature, no polymerization was observed. Only when the temperature was raised to normal thermal free radical polymerization temperatures, e.g., above 50°C-65°C, did polymerization occur, which resulted in a final polymer with a uniform structure.

[0148] Example 6. Redox-active SIS (FeCl 2 ) and stabilized SIS (FeCl 3 )’s synergistic impact.

[0149] The potential synergistic benefit of applying both redox-active SIS and stabilized SIS in staged polymerization was demonstrated. 3 (with different loading levels) were added to the prepolymerization mixture, followed by the addition of the redox active SIS FeCl 2 (with a fixed loading level) to initiate the polymerization process at ice bath temperature. After forming the first stage at low temperature, the second and third stages can be achieved by gradually increasing the polymerization temperature to conventional thermal free radical polymerization temperatures, such as above 50°C-65°C. Table 7 clearly shows that synergistic benefits can be achieved by mixing both stable and redox active SIS in a staged polymerization process.

[0150] Table 7. Redox activity of SIS (FeCl 2 ) and stabilized SIS (FeCl 3 )’s synergistic impact.

[0151]

[0152]

[0153] Example 7. Comparison of mechanical properties.

[0154] Compared to homogeneously cross-linked SAMs, staged SAMs have unique swelling kinetics. The different cross-linking densities in stage 1 and stage 2 exhibit a transition in mechanical strength during swelling in saline solution. When the liquid reaches the lower cross-linking density domain, especially inside the SAM particles, it is expected that the mechanical strength will drop during swelling. By design, this will be more profound for less or no cross-linker in stage 1.

[0155] Gel strength measuring instruments such as ElastoSens TM Bio Instruments can be used to measure the mechanical properties of SAM particles during dynamic swelling.

[0156] The following procedure was used for sample measurement. 0.1 g of SAM particles were placed on the ElastoSense TM The sample cup is then placed in the ElastoSense TM 5 mL of 0.9% NaCl solution was added to the sample cup and free swelling kinetics were recorded at 30 second intervals from 30 minutes to 1 hour.

[0157] Storage modulus data for polymers produced by staged polymerization and polymers not produced by staged polymerization are given in Figure 4 The polymer produced by staged polymerization exhibits an initial decrease in storage modulus caused by the liquid reaching the low crosslink density regions on the particle surface, and a large decrease in storage modulus between 300 and 500 seconds caused by the liquid reaching the low crosslink density regions inside the particles. In contrast, the polymer not produced by staged polymerization exhibits an initial increase in storage modulus, and no large decrease in storage modulus between 300 and 500 seconds.

[0158] In particular, the superabsorbent polymer produced by staged polymerization provides a 5.2% reduction in storage modulus (G') from about 883 Pa to about 837 Pa over a period of about 360 seconds to about 480 seconds. The superabsorbent polymer not produced by staged polymerization only provides a 1.5% reduction in storage modulus (G') from about 882 Pa to about 869 Pa over a period of about 330 seconds to about 390 seconds.

[0159] Additional storage modulus data for polymers produced by staged polymerization are available in Figure 5 The polymer produced by staged polymerization exhibits an initial decrease in storage modulus caused by the liquid reaching the low crosslink density regions on the particle surface, and a large decrease in storage modulus between 300 and 500 seconds caused by the liquid reaching the low crosslink density regions in the interior of the particle.

[0160] In particular, the superabsorbent polymer produced by staged polymerization provides a 10.8% reduction in storage modulus (G') from about 983 Pa to about 876.5 Pa over a period of about 330 seconds to about 450 seconds.

[0161] This written description uses examples to illustrate the disclosure, including the best mode, and also to enable any person skilled in the art to practice the disclosure, including making and using any compositions or systems and performing any included methods. The patentable scope of the disclosure is defined by the claims, and may include other examples that occur to those skilled in the art. Such other examples are intended to be within the scope of the claims if they have elements that do not differ from the literal language of the claims, or if they have equivalent elements with insubstantial differences from the literal language of the claims.

[0162] As used herein, the terms "comprises," "comprising," "includes," "including," "has," "having," "contains," "containing," "characterized by," or any other variation thereof, are intended to cover a non-exclusive inclusion, subject to any expressly indicated limitation. For example, a composition, mixture, process, or method that comprises a list of elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, mixture, process, or method.

[0163] The transitional phrase "consisting of" excludes any element, step, or ingredient not specified. If in a claim, this would approximate the claim to include materials other than those listed in addition to the impurities normally associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim, rather than immediately following a preamble, it is limited only to the elements set forth in that clause; other elements are not excluded from the claim as a whole.

[0164] The transitional phrase "consisting essentially of is used to define a composition or method that includes materials, steps, features, components, or elements in addition to those literally disclosed, provided that these additional materials, steps, features, components, or elements do not materially affect the basic and novel characteristics of the claimed invention. The term "consisting essentially of occupies the middle ground between "comprising" and "consisting of."

[0165] When an invention or a portion thereof is defined using open-ended terms such as "comprising," it should be readily understood that (unless otherwise indicated) the specification should be interpreted as also describing such an invention using the terms "consisting essentially of" or "consisting of."

[0166] In addition, unless expressly stated to the contrary, "or" refers to an inclusive or rather than an exclusive or. For example, a condition A or B is satisfied by any of the following: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist).

[0167] In addition, the indefinite articles "a" and "an" before an element or component of the present invention are intended to be non-restrictive with respect to the number of instances (i.e., occurrences) of the element or component. Therefore, "a" or "an" should be understood to include one or at least one, and the singular word form of an element or component also includes the plural unless the number is obviously intended to be singular.

[0168] As used herein, the term "about" means plus or minus 10% of a value.

Claims

1. A superabsorbent polymer, comprising: A polymer backbone, the polymer backbone comprising: Neutralized backbone monomers; a neutralized backbone monomer complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2; optional unneutralized backbone monomers; and optionally an unneutralized backbone monomer complexed with a coordination complex comprising a metal ion having an oxidation state of at least 2; and optional cross-linking agent; The superabsorbent polymer comprises a non-uniform microstructure.

2. The superabsorbent polymer of claim 1, wherein the superabsorbent polymer is configured to provide at least a 5.2% decrease in storage modulus (G') between 300 seconds and 500 seconds after exposure to a 0.9% NaCl solution at room temperature.

3. The superabsorbent polymer of claim 1, wherein the superabsorbent polymer comprises a core-shell polymer microstructure.

4. The superabsorbent polymer of claim 1, wherein the superabsorbent polymer comprises a first polymer portion having a first crosslink density and a second polymer portion having a second crosslink density, wherein the first crosslink density and the second crosslink density are different.

5. The superabsorbent polymer of claim 1, wherein the superabsorbent polymer comprises a first polymer fraction present in an amount ranging from about 1 to about 30 weight percent of the superabsorbent polymer and a second polymer fraction present in an amount ranging from about 60 to about 99 weight percent of the superabsorbent polymer.

6. The super absorbent polymer of claim 1, wherein the super absorbent polymer is in a form selected from the group consisting of particles, gels, fibers, beads, liquids, solids, pastes, or combinations thereof.

7. The superabsorbent polymer of claim 1, wherein the superabsorbent polymer is in the form of particles having a diameter ranging from about 100 μm to about 1000 μm.

8. A method for preparing a superabsorbent polymer, the method comprising: The initial polymerization stage includes forming a mixture comprising Solvents; monomer; salts comprising redox-active metal ions; optional cross-linking agent; as well as initiator; and reacting the mixture at a first temperature; and The final polymerization stage comprises optionally adding a cross-linking agent to the mixture; heating the mixture from the first temperature to a second temperature; as well as The mixture is reacted at the second temperature.

9. The method of claim 8, further comprising at least one intermediate polymerization stage between the initial polymerization stage and the final polymerization stage.

10. The method of claim 9, wherein the at least one intermediate polymerization stage comprises a time-dependent transition or a temperature-dependent transition.

11. The method of claim 10, wherein the at least one intermediate polymerization stage comprises adding a cross-linking agent to the mixture.

12. The method of claim 8, wherein the mixture further comprises a stable salt comprising a metal ion having an oxidation state of at least 2.

13. The process of claim 8, wherein the process comprises a plurality of polymerization stages ranging from 2 to 5.

14. The method of claim 8, wherein the first temperature is in the range of about -20°C to about 40°C.

15. The method of claim 8, wherein the second temperature is in the range of about 40°C to about 70°C.

16. The method of claim 8, wherein the method further comprises drying the reaction product.

17. The method of claim 8, further comprising grinding the reaction product.

18. A method of using a superabsorbent polymer, the superabsorbent polymer comprising A polymer backbone, the polymer backbone comprising: Neutralized backbone monomers; a neutralized backbone monomer complexed with a coordination complex comprising a metal ion in an oxidation state of at least 2; optional unneutralized backbone monomers; and optionally an unneutralized backbone monomer complexed with a coordination complex comprising a metal ion having an oxidation state of at least 2; and optional cross-linking agent; Wherein the superabsorbent polymer comprises a non-uniform microstructure and the method comprises using the superabsorbent polymer in a consumer product.

19. The method of claim 18, wherein the superabsorbent polymer is in the form of particles having a diameter ranging from about 100 μm to about 1000 μm.

20. The method of claim 18, wherein the consumer product is selected from the group consisting of personal hygiene products, wipes, napkins, bibs, disposable bed covers, wound dressings, food packaging, infant and adult diaper products, children's training pants, feminine pads and napkins, armbands, agricultural and pet products containing superabsorbent components, disposable absorbent products, and combinations thereof.

Citation Information

Patent Citations

  • Superabsorbent polymers having a slow rate of absorption

    CN102229686A

  • Copolymerized superabsorbent polymers

    CN116438209A

  • Crosslinked polymer, process for producing same, absorbent structure and absorbent article

    CN1441813A

  • Method for preparing high hydroscopicity resin by adding water-adsorbing resin for capturing polyvalent metal ion to unsaturated monomer water solution

    CN1970594A

  • Preparation Method of Super Absorbent Polymer

    US20210229070A1