Molybdenum ore flotation collecting agent and preparation method and application thereof
Through the synergistic use of organic oil, polymethoxydimethyl ether, C6 branched alcohols and non-ionic surfactants, a high-efficiency molybdenum ore flotation collector is formed, which solves the problem of poor effectiveness of traditional molybdenum ore flotation collectors. The recovery of high-efficiency molybdenum concentrate and environmental improvement are achieved.
Patent Information
- Application Number
- CN202411247373.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-10-25
AI Technical Summary
Traditional molybdenum ore flotation collectors such as diesel or kerosene result in huge drug consumption, low recovery rates, and serious environmental pollution, making it difficult to achieve efficient recovery of molybdenum sulfide concentrates.
The synergistic use of organic oil, polymethoxydimethyl ether, C6 branched alcohol and non-ionic surfactant is used to form a molybdenum ore flotation collector, which improves the selectivity and selectivity of molybdenum sulfide ore through its unique chemical properties and functions. Recovery rate.
The molybdenum grade in the molybdenum concentrate is ≥50.07% and the recovery rate is ≥87.10%. It overcomes the problems of high chemical consumption, strong odor and environmental pollution of traditional collectors, and improves resource utilization efficiency and operating environment safety.
Smart Images

Figure BDA0005031188350000021 
Figure BDA0005031188350000051 
Figure FDA0005031188340000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mineral processing, and in particular to a molybdenum ore flotation collector and a preparation method and application thereof. Background Art
[0002] At present, diesel or kerosene is traditionally widely used as a collector in the beneficiation process of molybdenum sulfide ore.
[0003] CN111167614A discloses a flotation method for sulfide copper-molybdenum ore. First, the copper-molybdenum ore is crushed, ground and deslimed to obtain a copper-molybdenum ore pulp with a concentration of 30-40%; then the copper-molybdenum ore pulp is added to a flotation device, and a collector kerosene and a foaming agent pine oil are added under a predetermined pH value condition to perform a mixed flotation process of first roughing, second concentrating, and second scavenging, and sequentially returning the ore to obtain a copper-molybdenum mixed concentrate; finally, the copper-molybdenum mixed concentrate is made into a mixed ore pulp with a concentration of 25-35%, adjusted to a predetermined pH value and a predetermined external control potential, and a copper inhibitor and / or a collector kerosene are added to perform a first roughing, a fourth concentrating, a second scavenging, and a second scavenging.
[0004] The flotation process of sweeping and sequentially returning the selected ores is used to separate the copper concentrate and molybdenum concentrate.
[0005] However, with the increasing awareness of resource conservation and environmental protection, the application bottlenecks of these traditional collectors have gradually emerged, and technological innovation is urgently needed. Specifically, the primary problem of using diesel or kerosene as collectors is the huge drug consumption, which directly leads to high production costs and is not conducive to the sustainable development of enterprises. Secondly, due to its limited collection performance, the recovery rate of molybdenum sulfide concentrate is difficult to significantly improve, and the resource utilization efficiency is not high. Third, the strong odor and large amount of volatile organic compounds released by diesel or kerosene during use not only seriously deteriorate the working environment and pose a potential threat to the health of operators, but also aggravate the problem of environmental pollution.
[0006] In summary, it can be seen that targeting molybdenum sulfide ore resources, developing a new and efficient molybdenum sulfide ore collector to achieve efficient flotation recovery of molybdenum sulfide resources has become a difficult problem to be solved urgently in the field of mineral processing. Summary of the invention
[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a molybdenum ore flotation collector and a preparation method and use thereof, so as to solve the problem that the currently used molybdenum ore flotation collector has poor flotation effect, resulting in poor concentrate grade and low recovery rate.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a molybdenum ore flotation collector, the molybdenum ore flotation collector comprising:
[0010] Organic oil, polyoxymethylene dimethyl ether, C6 branched alcohol and nonionic surfactant.
[0011] The molybdenum ore flotation collector provided by the present invention, through the coordinated use of organic oil, polymethoxy dimethyl ether, C6 branched alcohol and non-ionic surfactant, acts together on the flotation process of molybdenum sulfide ore through their unique chemical properties and functions, has good selectivity for molybdenum sulfide ore, avoids inclusion of other minerals such as pyrite, and realizes efficient recovery of molybdenum sulfide minerals.
[0012] As a preferred technical solution of the present invention, the molybdenum ore flotation collector comprises, by weight:
[0013]
[0014] As a preferred technical solution of the present invention, the organic oil includes one or a combination of at least two of diesel, biodiesel, kerosene or biokerosene.
[0015] Preferably, the C6 branched alcohol includes one or a combination of at least two of methyl isobutyl carbinol, diacetone alcohol or hexylene glycol.
[0016] Preferably, the nonionic surfactant includes fatty alcohol polyoxyethylene ether and / or alkylphenol polyoxyethylene ether.
[0017] As a preferred technical solution of the present invention, the organic oil is biodiesel.
[0018] Preferably, the C6 branched alcohol is methyl isobutyl carbinol.
[0019] Preferably, the nonionic surfactant is fatty alcohol polyoxyethylene ether.
[0020] Preferably, the degree of polymerization of the polyoxymethylene dimethyl ether is 3-8.
[0021] Preferably, the carbon chain of the fatty alcohol polyoxyethylene ether is C7-C9.
[0022] Preferably, the degree of polymerization of the fatty alcohol polyoxyethylene ether is 5-8.
[0023] In a second aspect, the present invention provides a method for preparing the molybdenum ore flotation collector as described in the first aspect, the preparation method comprising:
[0024] The ingredients are prepared according to the weight ratio, and the organic oil, polyoxymethylene dimethyl ether, C6 branched alcohol and non-ionic surfactant are mixed to obtain a molybdenum ore flotation collector.
[0025] As a preferred technical solution of the present invention, stirring is performed for 30-60 minutes during the mixing.
[0026] In a third aspect, the present invention provides a use of the molybdenum ore flotation collector as described in the first aspect, the use comprising:
[0027] The molybdenum ore flotation collector is used to flot the molybdenum ore.
[0028] As a preferred technical solution of the present invention, the -0.074 mm particle size material in the molybdenum ore accounts for 55-80% of the total mass of the material.
[0029] Preferably, the mass concentration of the ore pulp used for flotation is 30-45%.
[0030] As a preferred technical solution of the present invention, the flotation includes at least one roughing selection, at least two scavenging selections and at least six cleaning selections.
[0031] As a preferred technical solution of the present invention, a pH adjuster, a foaming agent and a collecting agent are added during the at least one rough selection.
[0032] Preferably, the pH adjuster used in the at least one rough selection comprises lime and / or sodium carbonate.
[0033] Preferably, the total amount of the pH adjuster added in the at least one rough selection is 100-500 g / t.
[0034] Preferably, the foaming agent used in the at least one rough selection comprises one or a combination of at least two of methyl isobutyl carbinol, pine oil or 2# oil.
[0035] Preferably, the total amount of the foaming agent used in the at least one rough selection is 20-100 g / t.
[0036] Preferably, the total amount of collector added in the at least one roughing is 30-150 g / t.
[0037] Preferably, the molybdenum ore flotation collector is added in the at least two sweeps.
[0038] Preferably, the addition amount of the molybdenum ore flotation collector used in the at least two sweeps is independently 5-20 g / t.
[0039] Preferably, a regulator is added during the at least six times of concentrating.
[0040] Preferably, the regulator used in the at least six times of beneficiation comprises water glass having a modulus of 2-3.
[0041] Preferably, the amount of the adjusting agent added in the at least six times of concentrating is independently 50-800 g / t.
[0042] Preferably, in the at least six times of cleaning, the -0.037 mm particle size material accounts for 80-90% of the total mass of the material.
[0043] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0044] The collector provided by the invention has high selectivity for molybdenum sulfide ore and strong collecting ability through the synergistic effect of biodiesel, polymethoxy dimethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether. The molybdenum grade in the molybdenum concentrate is ≥50.07%, and the recovery rate is ≥87.10%. The disadvantages of traditional diesel, kerosene and the like in the molybdenum recovery process, such as large agent consumption, strong odor, high emission of volatile organic compounds, low recovery rate, etc., are overcome, and the working environment is improved. DETAILED DESCRIPTION
[0045] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0046] This embodiment provides a molybdenum ore flotation collector, the molybdenum ore flotation collector comprising:
[0047] Organic oil, polyoxymethylene dimethyl ether, C6 branched alcohol and nonionic surfactant.
[0048] Specifically, the molybdenum ore flotation collector comprises, by weight:
[0049]
[0050]
[0051] In the present invention, the organic oil in the mineral flotation collector is 40-60 parts by weight, for example, it can be 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts, 46 parts, 47 parts, 48 parts, 49 parts, 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts or 60 parts, but is not limited to the listed values, and other unlisted values within the range also meet the requirements. If the weight part is less than 40 parts, the collection capacity becomes weak and the recovery rate of molybdenum concentrate is reduced; if the weight part is greater than 60 parts, it is not conducive to the recovery of difficult-to-select molybdenum.
[0052] In the present invention, the polyoxymethylene dimethyl ether in the mineral flotation collector is 15-35 parts by weight, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts or 35 parts, but is not limited to the listed values, and other unlisted values within the range also meet the requirements. If the weight part is less than 15 parts, the collecting ability of the collector becomes weak; if the weight part is greater than 35 parts, the foam viscosity becomes large, affecting the concentrate grade.
[0053] In the present invention, the C6 branched alcohol in the mineral flotation collector is 5-10 parts by weight, for example, it can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts, but is not limited to the listed values. Other unlisted values within this range also meet the requirements. If the weight is less than 5 parts, the foaming ability becomes weak, the collecting ability decreases, and the recovery rate of molybdenum is low; if the weight is greater than 10 parts, the foam viscosity becomes large, affecting the grade of the concentrate.
[0054] In the present invention, the nonionic surfactant in the mineral flotation collector is 1-3 parts by weight, for example, it can be 1 part, 1.5 parts, 2 parts, 2.5 parts or 3 parts, but it is not limited to the listed values. Other unlisted values within this range also meet the requirements. If the weight part is less than 1 part, the solubility, fluidity and dispersibility of the collector will deteriorate; if the weight part is greater than 3 parts, the amount of flotation foam will be large and the flotation process will be difficult to control.
[0055] Specifically, the organic oil includes one or a combination of at least two of diesel, biodiesel, kerosene or biokerosene, preferably biodiesel.
[0056] Preferably, the degree of polymerization of the polyoxymethylene dimethyl ether is 3-8, for example, 3, 4, 5, 6, 7 or 8, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0057] Specifically, the C6 branched alcohol includes one or a combination of at least two of methyl isobutyl carbinol, diacetone alcohol or hexylene glycol, preferably methyl isobutyl carbinol.
[0058] Specifically, the nonionic surfactant includes fatty alcohol polyoxyethylene ether and / or alkylphenol polyoxyethylene ether, preferably fatty alcohol polyoxyethylene ether.
[0059] Wherein, the carbon chain of the fatty alcohol polyoxyethylene ether is C7-C9.
[0060] In the present invention, the carbon chain of the fatty alcohol polyoxyethylene ether may be a straight chain hydrocarbon group or a branched hydrocarbon group.
[0061] The degree of polymerization of the fatty alcohol polyoxyethylene ether is 5-8, for example, 5, 6, 7 or 8, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0062] In the present invention, by combining organic oil, polymethoxy dimethyl ether, C6 branched alcohol and nonionic surfactant, with the help of the synergistic effect of each material in the component, the collector has good selectivity for molybdenum sulfide ore and avoids inclusion of other minerals such as pyrite; wherein, when organic oil, polymethoxy dimethyl ether, C6 branched alcohol and nonionic surfactant are used in combination, they act through a synergistic mechanism to improve the capture efficiency of molybdenum sulfide, and the unsaturated fatty acids in organic oil such as biodiesel can be selectively adsorbed on the surface of molybdenum minerals, and the adsorbed fatty acid molecules can change the hydrophilicity and hydrophobicity of the mineral surface, making the mineral surface more hydrophobic; polymethoxy dimethyl ether promotes the surface of molybdenum sulfide minerals through its oxygen-containing characteristics. Oxidation reaction increases the hydrophobicity of the mineral surface, which is beneficial to the attachment and separation of mineral particles and bubbles; C6 branched alcohols such as methyl isobutyl carbinol can produce a stable and easy-to-control foam layer, which provides the necessary buoyancy and separation space for the flotation of molybdenum sulfide mineral particles, helps to separate molybdenum sulfide mineral particles from gangue minerals, and improves the selectivity and recovery rate of the flotation process; non-ionic surfactants such as fatty alcohol polyoxyethylene ether have excellent dispersing, emulsifying, wetting and penetrating properties, and can evenly disperse the components of the collector system in the solution to form a stable emulsion or dispersion system, making it easier for the collector to penetrate into the fine structure of the mineral and enhancing the adsorption of the collector on the surface of the molybdenum sulfide ore.
[0063] In summary, the synergistic use of organic oil, polyoxymethylene dimethyl ether, C6 branched alcohol and non-ionic surfactant, through their unique chemical properties and functions, jointly acts on the flotation process of molybdenum sulfide ore to achieve efficient recovery of molybdenum sulfide minerals.
[0064] Furthermore, the present invention provides a method for preparing the molybdenum ore flotation collector as described above, the preparation method comprising:
[0065] The ingredients are prepared according to the weight ratio, and the organic oil, polyoxymethylene dimethyl ether, C6 branched alcohol and non-ionic surfactant are mixed to obtain a molybdenum ore flotation collector.
[0066] Specifically, the mixing is stirred for 30-60 min, for example, 30 min, 32 min, 34 min, 36 min, 38 min, 40 min, 42 min, 44 min, 46 min, 48 min, 50 min, 52 min, 54 min, 56 min, 58 min or 60 min, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0067] Furthermore, the present invention provides the use of the molybdenum ore flotation collector as described above, the use comprising:
[0068] The molybdenum ore flotation collector is used to flot the molybdenum ore.
[0069] Specifically, the -0.074 mm particle size material in the molybdenum ore accounts for 55-80% of the total mass of the material, for example, it can be 55%, 60%, 65%, 70%, 75% or 80%, etc., but is not limited to the listed values, and other unlisted values within this range also meet the requirements.
[0070] Specifically, the mass concentration of the ore pulp used for flotation is 30-45%, for example, it can be 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44% or 45%, etc., but is not limited to the listed values, and other unlisted values within this range also meet the requirements.
[0071] Specifically, the flotation comprises at least one roughing separation, at least two scavenging separations and at least six cleaning separations.
[0072] In the present invention, the middlings obtained by scanning and concentration are sequentially returned to the previous operation for continued selection, such as the middlings obtained by concentration are returned to the previous concentration operation.
[0073] Specifically, a pH adjuster, a foaming agent and a collecting agent are added during the at least one rough selection.
[0074] Specifically, the pH adjuster used in the at least one rough selection includes lime and / or sodium carbonate.
[0075] Specifically, the amount of the pH adjuster used in the at least one rough selection is 100-500 g / t, for example, 100 g / t, 200 g / t, 300 g / t, 400 g / t or 500 g / t, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0076] In the present invention, the amount of pH adjuster added in at least one rough selection is the total amount added, and the amount added each time can be reasonably allocated according to actual needs.
[0077] Specifically, the foaming agent used in the at least one rough selection includes one or a combination of at least two of methyl isobutyl carbinol, pine oil or 2# oil.
[0078] Specifically, the addition amount of the foaming agent used in the at least one rough selection is 20-100 g / t, for example, it can be 20 g / t, 30 g / t, 40 g / t, 50 g / t, 60 g / t, 70 g / t, 80 g / t, 90 g / t or 100 g / t, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0079] In the present invention, the amount of the foaming agent used in at least one rough selection is the total amount of addition, and the amount of addition corresponding to each time can be reasonably allocated according to actual needs.
[0080] Specifically, the addition amount of the collector used in the at least one rough selection is 30-150 g / t, for example, it can be 30 g / t, 40 g / t, 60 g / t, 80 g / t, 100 g / t, 120 g / t, 140 g / t or 150 g / t, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0081] In the present invention, the amount of collector used in at least one rough selection is the total amount, and the amount added each time can be reasonably allocated according to actual needs.
[0082] Specifically, the molybdenum ore flotation collector is added in the at least two sweeps.
[0083] Wherein, the addition amount of the molybdenum ore flotation collector used in each sweep is independently 5-20 g / t, for example, it can be 5 g / t, 6 g / t, 7 g / t, 8 g / t, 9 g / t, 10 g / t, 11 g / t, 12 g / t, 13 g / t, 14 g / t, 15 g / t, 16 g / t, 17 g / t, 18 g / t, 19 g / t or 20 g / t, etc., for example, it can be 15 g / t, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0084] Specifically, a regulator is added during the at least six times of concentrating.
[0085] Specifically, the regulator used in the at least six times of beneficiation includes water glass.
[0086] In the present invention, the modulus of the water glass used is 2-3.
[0087] Specifically, the addition amount of the adjuster used in the at least six times of selection is independently 50-800 g / t, for example, it can be 50 g / t, 60 g / t, 80 g / t, 100 g / t, 200 g / t, 300 g / t, 400 g / t, 500 g / t, 600 g / t, 700 g / t or 800 g / t, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0088] In the present invention, the amount of the adjusting agent added in at least six rounds of concentrating is the amount of the adjusting agent added in a single round of concentrating.
[0089] Specifically, in the at least six times of selection, the -0.037mm particle size material accounts for 80-90% of the total mass of the material, for example, it can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89% or 90%, etc., but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0090] In the present invention, the unit of addition amount "g / t" means that a certain amount of reagent is added per t of raw ore.
[0091] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0092] Further, in order to illustrate that the molybdenum ore flotation collector provided by the present invention can achieve good flotation collection effect in the flotation process, the following actual examples are used for illustration, as follows:
[0093] Example 1
[0094] The present invention provides a molybdenum ore flotation collector, the molybdenum ore flotation collector comprising:
[0095] 50 parts of biodiesel, 30 parts of polyoxymethylene ether (polymerization degree is 5), 8 parts of methyl isobutyl carbinol and 2 parts of fatty alcohol polyoxyethylene ether (JFC-2).
[0096] The specific preparation process is as follows:
[0097] According to the formula, biodiesel, polyoxymethylene dimethyl ether and methyl isobutyl carbinol are mixed at normal temperature and pressure, and fatty alcohol polyoxyethylene ether is added and stirred for 45 minutes to obtain a molybdenum ore flotation collector.
[0098] Example 2
[0099] The present invention provides a molybdenum ore flotation collector, the molybdenum ore flotation collector comprising:
[0100] 55 parts of biodiesel, 28 parts of polyoxymethylene ether (polymerization degree is 6), 7 parts of methyl isobutyl carbinol and 1.5 parts of fatty alcohol polyoxyethylene ether (JFC-2).
[0101] The specific preparation process is as follows:
[0102] According to the formula, biodiesel, polyoxymethylene dimethyl ether and methyl isobutyl carbinol are mixed at normal temperature and pressure, and fatty alcohol polyoxyethylene ether is added and stirred for 30 minutes to obtain the collector.
[0103] Example 3
[0104] The present invention provides a molybdenum ore flotation collector, the molybdenum ore flotation collector comprising:
[0105] 45 parts of biodiesel, 35 parts of polyoxymethylene ether (polymerization degree is 5), 9 parts of methyl isobutyl carbinol and 1 part of fatty alcohol polyoxyethylene ether (JFC-2).
[0106] The specific preparation process is as follows:
[0107] According to the formula, biodiesel, polyoxymethylene dimethyl ether and methyl isobutyl carbinol are mixed at normal temperature and pressure, and fatty alcohol polyoxyethylene ether is added and stirred for 55 minutes to obtain the collector.
[0108] Example 4
[0109] The present invention provides a molybdenum ore flotation collector, the molybdenum ore flotation collector comprising:
[0110] 60 parts of biodiesel, 25 parts of polyoxymethylene ether (polymerization degree is 6), 7 parts of methyl isobutyl carbinol and 2 parts of fatty alcohol polyoxyethylene ether (JFC-2).
[0111] The specific preparation process is as follows:
[0112] According to the formula, biodiesel, polyoxymethylene dimethyl ether and methyl isobutyl carbinol are mixed at normal temperature and pressure, and fatty alcohol polyoxyethylene ether is added and stirred for 40 minutes to obtain a molybdenum ore flotation collector.
[0113] Example 5
[0114] The only difference from Example 1 is that the weight portion of biodiesel in the collector is 80 parts.
[0115] Example 6
[0116] The only difference from Example 1 is that the weight proportion of polyoxymethylene dimethyl ether in the collector is 50 parts.
[0117] Example 7
[0118] The only difference from Example 1 is that the weight parts of methyl isobutyl carbinol in the collector is 20 parts.
[0119] Example 8
[0120] The only difference from Example 1 is that the weight proportion of fatty alcohol polyoxyethylene ether in the collector is 8 parts.
[0121] Example 9
[0122] The only difference from Example 1 is that the biodiesel in the collector is replaced with an equal amount of diesel.
[0123] Example 10
[0124] The only difference from Example 1 is that the fatty alcohol polyoxyethylene ether in the collector is replaced with an equal amount of alkylphenol polyoxyethylene ether (NP-10).
[0125] Comparative Example 1
[0126] The only difference from Example 1 is that no polyoxymethylene dimethyl ether is added to the collector.
[0127] Comparative Example 2
[0128] The only difference from Example 1 is that methyl isobutyl carbinol is not added to the collector.
[0129] Comparative Example 3
[0130] The only difference from Example 1 is that no fatty alcohol polyoxyethylene ether is added to the collector.
[0131] Comparative Example 4
[0132] The only difference from Example 1 is that the methyl isobutyl carbinol in the collector is replaced by an equal amount of 2# oil.
[0133] Comparative Example 5
[0134] The only difference from Example 1 is that the polyoxymethylene dimethyl ether in the collector is replaced by an equal amount of diesel.
[0135] Example 6
[0136] The only difference from Example 1 is that the polyoxymethylene dimethyl ether in the collector is replaced by an equal amount of kerosene.
[0137] Comparative Example 7
[0138] The only difference from Example 1 is that the polyoxymethylene dimethyl ether in the collector is replaced by an equal amount of N,N-diethyldithiocarbamate propionitrile.
[0139] Comparative Example 8
[0140] This comparative example provides a collector, which is diesel.
[0141] Comparative Example 9
[0142] This comparative example provides a collector, which is kerosene.
[0143] The flotation performance test of the collector provided in the above embodiment and comparative example on sulfide molybdenum ore is as follows: the raw ore of a certain sulfide molybdenum ore (Mo content 0.12%) is ground to a mass percentage of 65% of the material of -0.074mm particle size, the pulp concentration is 40%, and a pH adjuster, a collector, and a frother are added to carry out a roughing process (lime addition amount is 300g / t, pine oil addition amount is 60g / t and molybdenum ore flotation collector is 90g / t), two scavenging processes (molybdenum ore flotation collector addition amount is 10g / t) and six times of concentrating treatment. Among them, when concentrating, the mass percentage of the material of the rough concentrate after grinding to a -0.037mm particle size is 85%, and the adjusting agent water glass (water glass with a modulus of 2.5, each addition amount is 300g / t), and the specific test results are shown in Table 1.
[0144] Table 1
[0145] Molybdenum concentrate grade (%) Recovery rate (%) Example 1 51.30 91.01 Example 2 51.17 90.66 Example 3 51.02 91.03 Example 4 50.59 90.90 Example 5 50.54 87.10 Example 6 50.77 87.99 Example 7 50.62 87.12 Example 8 50.07 87.54 Example 9 50.47 88.52 Example 10 50.67 87.88 Comparative Example 1 50.53 87.55 Comparative Example 2 50.45 87.27 Comparative Example 3 50.71 88.07 Comparative Example 4 50.12 87.86 Comparative Example 5 50.16 87.20 Comparative Example 6 50.82 87.16 Comparative Example 7 50.17 85.54 Comparative Example 8 50.46 87.18 Comparative Example 9 50.77 86.41
[0146] It can be seen from the above table that the collector provided by the present invention can enhance the recovery of molybdenum sulfide by compounding biodiesel, polymethoxy dimethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether. The molybdenum grade in the molybdenum concentrate is ≥50.07%, and the molybdenum recovery rate is ≥87.10%. Under the preferred embodiment, the molybdenum grade in the obtained molybdenum concentrate is ≥50.59%, and the molybdenum recovery rate is ≥90.66%.
[0147] Comparison of Examples 1-4 with Examples 5-8 shows that biodiesel, polyoxymethylene ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether have better recovery effects on molybdenum sulfide ore within a specific content range.
[0148] By comparing Example 1 with Examples 9-10, it can be seen that when the preferred scheme of the present invention is used to combine collectors such as biodiesel, polyoxymethylene ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether, a more excellent flotation collection effect is achieved.
[0149] By comparing Example 1 with Comparative Examples 1-9, it can be seen that compared with conventional collectors, the collector adopts the specific combination of the present invention, and the grade and recovery rate of the molybdenum concentrate obtained by flotation are improved. When a certain component is removed or a certain component is replaced by other agents, the molybdenum grade or molybdenum recovery rate in the molybdenum concentrate decreases.
[0150] In summary, the collector provided by the present invention forms a specific ratio of biodiesel, polymethoxydimethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether, which can not only improve the grade and recovery rate of molybdenum concentrate, but also overcome the disadvantages of traditional diesel, kerosene and the like in the molybdenum recovery process, such as large consumption of reagents, strong odor, high emission of volatile organic compounds, low recovery rate, etc., and provides a new way for the efficient development and utilization of sulfide molybdenum ore resources.
[0151] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0152] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0153] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A molybdenum ore flotation collector, It is characterized in that The molybdenum ore flotation collector comprises: Organic oil, polyoxymethylene dimethyl ether, C6 branched alcohol and nonionic surfactant.
2. The molybdenum ore flotation collector according to claim 1, It is characterized in that The molybdenum ore flotation collector comprises, by weight:
3. The molybdenum ore flotation collector according to claim 1, It is characterized in that The organic oil comprises one or a combination of at least two of diesel, biodiesel, kerosene or biokerosene; Preferably, the C6 branched alcohol comprises one or a combination of at least two of methyl isobutyl carbinol, diacetone alcohol or hexylene glycol; Preferably, the nonionic surfactant includes fatty alcohol polyoxyethylene ether and / or alkylphenol polyoxyethylene ether.
4. The molybdenum ore flotation collector according to claim 1, It is characterized in that The organic oil is biodiesel; Preferably, the C6 branched alcohol is methyl isobutyl carbinol; Preferably, the nonionic surfactant is fatty alcohol polyoxyethylene ether; Preferably, the degree of polymerization of the polyoxymethylene dimethyl ether is 3-8; Preferably, the carbon chain of the fatty alcohol polyoxyethylene ether is C7-C9; Preferably, the degree of polymerization of the fatty alcohol polyoxyethylene ether is 5-8.
5. A method for preparing a molybdenum ore flotation collector according to any one of claims 1 to 4, It is characterized in that The preparation method comprises: The ingredients are prepared according to the weight ratio, and the organic oil, polyoxymethylene dimethyl ether, C6 branched alcohol and non-ionic surfactant are mixed to obtain a molybdenum ore flotation collector.
6. The preparation method according to claim 5, It is characterized in that The mixture is stirred for 30-60 min.
7. Use of a molybdenum ore flotation collector as claimed in any one of claims 1 to 4, It is characterized in that The uses include: The molybdenum ore flotation collector is used to flot the molybdenum ore.
8. The use according to claim 7, It is characterized in that The -0.074 mm particle size material in the molybdenum ore accounts for 55-80% of the total mass of the material; Preferably, the mass concentration of the ore pulp used for flotation is 30-45%.
9. The use according to claim 7, It is characterized in that The flotation comprises at least one roughing process, at least two scavenging processes and at least six cleaning processes.
10. The use according to claim 9, It is characterized in that A pH adjuster, a frother and a collector are added in at least one rough selection; Preferably, the pH adjuster used in the at least one rough selection comprises lime and / or sodium carbonate; Preferably, the total amount of the pH adjuster used in the at least one rough selection is 100-500 g / t; Preferably, the foaming agent used in the at least one rough selection includes one or a combination of at least two of methyl isobutyl carbinol, pine oil or 2# oil; Preferably, the total amount of the foaming agent used in the at least one rough selection is 20-100 g / t; Preferably, the total amount of collector used in the at least one rough selection is 30-150 g / t; Preferably, the molybdenum ore flotation collector is added in the at least two sweeps; Preferably, the addition amount of the molybdenum ore flotation collector used in the at least two sweeps is independently 5-20 g / t; Preferably, an adjusting agent is added during the at least six times of concentrating; Preferably, the adjusting agent used in the at least six times of selection comprises water glass having a modulus of 2-3; Preferably, the amount of the adjusting agent added in the at least six times of concentrating is independently 50-800 g / t; Preferably, in the at least six times of cleaning, the -0.037 mm particle size material accounts for 80-90% of the total mass of the material.