Copper-zirconium intermediate alloy core-spun tube as well as preparation method and application thereof
Through the preparation and wire feeding control of copper-zirconium master alloy core-clad tubes, the problems of oxidation and particle leakage of copper-chromium-zirconium alloys in high-temperature smelting and casting are solved, the uniform distribution and large-scale production of copper-zirconium alloys are achieved, and the loss of zirconium is reduced. Oxidation losses improve production quality.
Patent Information
- Application Number
- CN202411086850.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Copper-chromium-zirconium alloys are prone to oxidation and volatilization during high-temperature smelting and casting, resulting in uneven composition and difficult to control under non-vacuum smelting, which limits production scale and cost, especially the oxidation loss of zirconium and particle leakage.
The copper-zirconium master alloy core-clad tube is used. By controlling the particle size and particle size, unalloyed or insufficiently alloyed elements are removed, and the core-clad tube is processed into a core-clad tube, and annealed under nitrogen protection, combined with PLC-controlled wire feeding. machine to achieve even distribution and rapid melting, reducing oxidation losses.
It achieves uniform and dense distribution of copper-zirconium alloy, reduces the oxidation loss of zirconium, improves production quality and large-scale production capacity, and ensures the composition stability of the cast slab and no air residue.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of copper alloys, and in particular relates to a copper-zirconium master alloy cored tube and a preparation method and application thereof. Background Art
[0002] Copper-chromium-zirconium alloy has good electrical conductivity, thermal conductivity, high hardness, wear resistance, explosion resistance, corrosion resistance, crack resistance and high softening temperature. This material is widely used in the manufacture of electrode materials for automatic welding machines for automobiles, large-scale integrated circuits, high-speed train contact lines, switch contact bridges and continuous casting steel crystallizers. In recent years, the demand for clean energy has grown rapidly, and copper-chromium-zirconium alloys are also widely used in electrolytic copper foil, solar photovoltaic panels, lithium batteries and other fields. In the future, with the continuous expansion of the new energy market, the application of copper-chromium-zirconium alloys in the field of new energy will increase further. Therefore, the copper-chromium-zirconium alloy industry is expected to usher in a broader development prospect in the future. However, the production technology of copper-chromium-zirconium alloy is relatively difficult, mainly because chromium and zirconium have a strong affinity with oxygen under high-temperature smelting and casting conditions, and are easily oxidized and volatilized during the smelting and casting process, resulting in uneven composition. Generally, vacuum melting and casting methods are required to reduce oxidation and volatilization to ensure that the final product has the required chemical composition. However, due to the structure of the vacuum induction furnace, its production method is limited to products with periodic operations. The weight or length of a single casting is limited by the capacity of the crucible, and it is impossible to produce products with a larger weight or theoretically unlimited length, and the production cost is high. Non-vacuum casting can produce products with a larger weight or theoretically unlimited length, but the problem of difficult control of composition under non-vacuum conditions must be solved. For example, zirconium in copper-zirconium master alloys is easily oxidized or particles are leaked, causing losses, and the temperature drop of copper liquid in the launder causes the copper liquid to solidify, which to a certain extent makes the composition unstable under non-vacuum conditions, affecting production.
[0003] Therefore, it is necessary to develop a copper-zirconium intermediate core tube that can reduce zirconium oxidation loss and achieve large-scale production and is used for non-vacuum smelting to manufacture copper-zirconium alloy. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a copper-zirconium master alloy cored tube and a preparation method and application thereof. The copper-zirconium master alloy cored wire has a low melting point, high reliability, and the copper-zirconium master alloy particles inside the cored wire are evenly and densely distributed without air residue. When used for non-vacuum smelting to manufacture copper-zirconium alloy, the melting speed is fast, the particles are evenly distributed and flow into a crystallizer to be cast into a casting billet, which can not only reduce the oxidation loss of zirconium, but also realize large-scale production.
[0005] In order to solve the technical problem proposed by the present invention, the present invention provides a copper-zirconium master alloy cored tube, comprising an inner core and a cladding, wherein the cladding is a T2 copper tube, and the inner core is a copper-zirconium master alloy particle, whose particle size is ≤1.0 mm, and does not contain unalloyed or insufficiently alloyed elements. In the technical solution, by controlling the particle size of the copper-zirconium master alloy particles and removing the unalloyed or insufficiently alloyed elements, after being processed into a copper-zirconium master alloy cored tube, the copper-zirconium master alloy particles in the copper tube meet the requirements of being dense, uniform, free of other impurity elements, and basically free of air residue, which can accelerate the melting speed, greatly reduce the oxidation and burning loss of zirconium, and add uniformly, which can improve the quality of subsequent copper casting.
[0006] Furthermore, the zirconium content in the copper-zirconium master alloy particles is 45-55%. The present invention selects a copper-zirconium master alloy with a zirconium content of 45-55% as a copper-zirconium alloy source, and its melting point is ≤950°C. After being fed into the launder copper liquid, it will melt immediately and evenly distribute in the copper liquid, and then gradually flow into the crystallizer in a short time to be cast into a casting billet, which can greatly reduce the oxidation and loss of zirconium.
[0007] The present invention also provides a method for preparing the copper-zirconium master alloy cored tube, comprising the following steps: (1) Prepare T2 copper tube and copper-zirconium master alloy for standby use, with the weight ratio between the two being between 0.35 and 1; (2) Crushing and screening: The purchased copper-zirconium master alloy is crushed and screened by a jaw crusher to separate and remove large particles with insufficient alloying, and to screen out master alloy particles with a particle size of ≤1.0 mm. By mechanically crushing and screening the copper-zirconium master alloy to remove large particles with insufficient alloying, the impurity content can be greatly reduced, the melting point is low, and the melting speed is fast; (3) Filling particles: The intermediate alloy particles obtained in step (2) are placed into the T2 copper tube, and air is expelled through a certain vibration to make the filling more dense; (4) Disc drawing: The copper tube filled with copper-chromium master alloy particles in step (3) is placed in a disc and drawn multiple times to reduce the outer diameter, increase the length, and completely squeeze out the residual gas; (5) Annealing: The copper tube drawn in step (4) is annealed under nitrogen protection to obtain a copper-zirconium master alloy core tube. Annealing under nitrogen protection can prevent oxidation of the copper-zirconium master alloy core tube and contamination by other impurities, while also improving its stability and uniformity.
[0008] Furthermore, in step (1), the ratio of the outer diameter to the wall thickness of the copper tube is between 10-28.
[0009] Furthermore, in step (4), the diameter reduction rate of the copper tube after drawing is 30-80%, and the single-pass diameter reduction rate is ≤20%. In this technical solution, by drawing the copper tube in multiple passes, the particles in the tube can be compacted and tight, avoiding leakage and separation of alloy particles during the subsequent wire feeding process, and further eliminating the air in the tube to reduce oxidation and burning; by controlling the drawing diameter reduction rate, the quality of the copper-chromium-zirconium alloy cored tube is improved.
[0010] Furthermore, in step (5), the annealing temperature is 350-550°C.
[0011] The present invention also provides an application of the copper-zirconium master alloy cored tube in non-vacuum melting and casting of copper-chromium-zirconium alloy large flat ingots, and the application method is as follows: S1. Copper smelting: Use coreless induction furnace to melt electrolytic copper plate. The melting process is completely covered with charcoal to prevent air from entering the copper liquid. The melting temperature is 1100-1200℃; S2. Argon degassing: After heating the molten copper to 1150-1200℃, let it stand for 5-15min, and introduce compressed argon gas to the bottom of the copper liquid through a graphite tube for 5-15min. The charcoal should be fully covered during the whole process. S3. Adding copper-chromium intermediate: After degassing, the temperature of the molten copper is raised to 1200-1250°C, and the copper-chromium intermediate alloy is added according to the alloy composition ratio to fully melt the alloy, and the temperature is maintained at 1200-1250°C, and the charcoal is fully covered; S4. Pour the molten copper: When the temperature of the molten copper reaches 1200-1250°C, open the graphite stopper rod, and the molten copper enters the launder equipped with an induction coil, and the launder induction coil heats the molten copper at high power; S5. Adding copper-zirconium master alloy cored tube: During the process of copper liquid filling the launder, start the wire feeder and add the copper-zirconium master alloy cored tube at a certain speed. The wire feeder speed is determined by the alloy composition ratio; S6. Casting: When the copper liquid fills 50-85% of the flow channel volume, the graphite stopper of the flow channel is opened, and the copper liquid enters the crystallizer for casting. At the same time, the copper liquid in the crystallizer is completely covered with carbon black powder to obtain an ingot.
[0012] Furthermore, in S4, the induction coil is installed in the middle of the launder, and the heating power during production is 0-30kW; before the copper liquid flows in, the launder is heated and baked with burning charcoal for 30-40 minutes in advance; the induction coil is baked with a low current. By installing the induction coil at the interruption part of the launder, it can be used to heat the launder, preventing the temperature drop of the copper liquid after it flows into the launder, which affects the subsequent production.
[0013] Furthermore, in S5, the wire feeder adopts PLC to control the speed, and is associated with the speed of the ingot casting machine; the wire feeding speed of the wire feeder is controlled according to the amount of Zr element in the ingot produced per unit time of 0.15%. The use of PLC to control the wire feeding speed can ensure that the copper-zirconium master alloy tube is added continuously, evenly and dynamically, reduce the oxidation and loss of zirconium, improve uniformity, and realize large-scale production.
[0014] Furthermore, in S6, the casting speed is 50-100 mm / min.
[0015] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: The invention strictly controls various processes from material selection to preparation, and the obtained copper-zirconium intermediate alloy tube is a seamless copper tube with few impurities, dense and uniform, no air residue, and low melting point. It is used for non-vacuum smelting to manufacture copper-zirconium alloy, and can reduce oxidation and loss of zirconium.
[0016] The present invention optimizes the ingot casting production process, and horizontally installs a group of induction coils in the middle section of the flow channel. During production, the copper liquid in the flow channel can be heated to prevent the copper liquid in the flow channel from cooling down and affecting the subsequent addition of the copper-zirconium master alloy tube. The wire feeding speed is controlled by PLC, and is associated with the speed of the ingot casting machine. Once the copper-zirconium master alloy tube touches the copper liquid, it is immediately melted and evenly distributed in the copper liquid, and then gradually flows into the crystallizer in a short time to be cast into a casting blank, so that the copper-zirconium master alloy tube can be continuously, evenly and dynamically added without leakage, and is used for large-scale production of copper-zirconium alloy by non-vacuum smelting. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. When the concentrations involved in the present invention are not specified, they are all mass concentrations. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0018] The chemical composition of copper-chromium master alloy is CuCr10.
[0019] The chemical composition of the copper-zirconium master alloy is CuZr50, and the particle size is ≤1mm.
[0020] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0021] Example 1 A method for preparing a copper-zirconium master alloy cored tube comprises the following steps: (1) Prepare a T2 copper tube and a copper-zirconium master alloy for standby use; wherein the outer diameter of the T2 copper tube is 28 mm and the wall thickness is 1.0 mm, the zirconium content in the copper-zirconium master alloy is 50%, and the weight ratio of the T2 copper tube to the copper-zirconium master alloy is 0.72; (2) Crushing and screening: The purchased copper-zirconium master alloy is crushed and screened by a jaw crusher to separate and remove large particles that are not fully alloyed, and to screen out master alloy particles with a particle size of ≤1.0 mm; (3) Filling particles: The intermediate alloy particles obtained in step (2) are placed into the T2 copper tube, and air is expelled through a certain vibration to make the filling more dense; (4) Disc drawing: The copper tube filled with copper-zirconium master alloy particles in step (3) is placed in a disc and drawn six times, and the tube diameters are 28 mm --> 22.95 mm --> 19.17 mm --> 16 mm --> 13.35 mm --> 11.2 mm --> 9.52 mm in sequence; (5) Annealing: The copper tube drawn in step (4) is annealed under nitrogen protection at a temperature of 450° C. to obtain a copper-zirconium master alloy core tube, which is a seamless copper tube with a dense cross section.
[0022] Example 2 A method for preparing a copper-zirconium master alloy cored tube comprises the following steps: (1) Prepare a T2 copper tube and a copper-zirconium master alloy for standby use; wherein the outer diameter of the T2 copper tube is 25 mm and the wall thickness is 1.0 mm, the zirconium content in the copper-zirconium master alloy is 50%, and the weight ratio of the T2 copper tube to the copper-zirconium master alloy is 1; (2) Crushing and screening: The purchased copper-zirconium master alloy is crushed and screened by a jaw crusher to separate and remove large particles that are not fully alloyed, and to screen out master alloy particles with a particle size of ≤1.0 mm; (3) Filling particles: The intermediate alloy particles obtained in step (2) are placed into the T2 copper tube, and air is expelled through a certain vibration to make the filling more dense; (4) Disc drawing: The copper tube filled with copper-zirconium master alloy particles in step (3) is placed in a disc and drawn six times, with the tube diameters being 25 mm --> 20.5 mm --> 17.12 mm --> 14.30 mm --> 11.94 mm --> 10.02 mm --> 8.52 mm in sequence; (5) Annealing: The copper tube drawn in step (4) is annealed under nitrogen protection at a temperature of 550° C. to obtain a copper-zirconium master alloy core tube, which is a seamless copper tube with a dense cross section.
[0023] Example 3 An application of a copper-zirconium master alloy cored tube in non-vacuum melting and casting of a copper-chromium-zirconium alloy large flat ingot, and the application method thereof is as follows: S1. Copper smelting: The electrolytic copper plate is melted in a coreless induction furnace. The melting process is completely covered with charcoal to prevent air from entering the copper liquid. The melting temperature is 1200℃. S2. Argon degassing: After heating the molten copper to 1200°C, let it stand for 5 minutes, and then introduce compressed argon gas to the bottom of the copper liquid through a graphite tube for 5 minutes. The charcoal should be fully covered during the whole process. S3. Adding copper-chromium master alloy: After degassing, the temperature of the molten copper is raised to 1250°C, and the copper-chromium master alloy is added according to the alloy composition ratio to fully melt the master alloy, and the temperature is maintained at 1250°C, and the charcoal is fully covered; S4. Pour the molten copper: When the temperature of the molten copper reaches 1250°C, open the graphite plug rod, and the molten copper enters the flow channel with an induction coil installed in the middle part, and the flow channel induction coil heats the molten copper at high power; S5. Adding the copper-zirconium master alloy cored tube obtained in Example 1: During the process of filling the trough with molten copper, the wire feeder is started, the speed is controlled by PLC, and is associated with the speed of the ingot casting machine. The speed of the wire feeder feeding the copper-zirconium master alloy cored tube is controlled according to the amount of Zr element in the ingot produced per unit time of 0.15%; S6. Casting: When the copper liquid fills 50% of the volume of the launder, the launder graphite stopper is opened, and the copper liquid enters the crystallizer and is cast at a speed of 50 mm / min. At the same time, the copper liquid in the crystallizer is completely covered with carbon black powder, and no water spraying is used for secondary cooling at the crystallizer outlet to obtain an ingot.
[0024] Comparative Example 1 A method for preparing a copper-zirconium master alloy cored tube comprises the following steps: (1) Prepare a T2 copper tube and a copper-zirconium master alloy for standby use; wherein the outer diameter of the T2 copper tube is 28 mm and the wall thickness is 0.6 mm, the zirconium content in the copper-zirconium master alloy is 50%, and the weight ratio of the T2 copper tube to the copper-zirconium master alloy is 1; (2) Crushing and screening: The purchased copper-zirconium master alloy is crushed and screened by a jaw crusher to separate and remove large particles that are not fully alloyed, and to screen out master alloy particles with a particle size of ≤1.0 mm; (3) Filling particles: The intermediate alloy particles obtained in step (2) are placed into the T2 copper tube, and air is expelled through a certain vibration to make the filling more dense; (4) Disc drawing: The copper tube filled with copper-zirconium master alloy particles in step (3) was placed in a disc and drawn six times as planned. However, when the Ø19.17 mm tube was stretched to the Ø16 mm tube, it frequently broke and could not be stretched.
[0025] Comparative Example 2 An application of a copper-zirconium master alloy cored tube in non-vacuum casting of a copper-chromium-zirconium alloy large flat ingot, and the application method thereof is as follows: The difference from Example 4 is that: S4: pouring the copper liquid: when the temperature of the copper liquid reaches 1200°C, open the graphite stopper; S5: Adding the copper-zirconium master alloy cored tube obtained in Example 1: During the process of filling the launder with molten copper, the wire feeder is started, and the speed of the wire feeder feeding the copper-zirconium master alloy cored tube is controlled according to the amount of Zr element in the ingot produced per unit time of 0.15%.
[0026] Comparative Example 3 During the casting process, a cored wire with a diameter of 6 mm wrapped with CuZr50 intermediate alloy powder and a wall thickness of 0.4 mm purchased from the market was continuously added to the flow channel at a speed matching the casting speed using a wire feeder. Other conditions were exactly the same as in Implementation Case 3.
[0027] Test example The chromium and zirconium contents in different parts of the ingots cast in Example 3 and Comparative Examples 2-3 were tested, and the results are shown in Table 1. The composition of the ingot was measured at intervals of 1 meter from the beginning to the end, wherein the maximum zirconium deviation % = (maximum zirconium content-minimum zirconium content) × 100 / average value of the zirconium content in each part.
[0028] Table 1 Content of chromium and zirconium in different parts of ingot
[0029] It can be seen from the results in Table 1 that the large flat ingot of copper-chromium-zirconium alloy prepared by the copper-zirconium master alloy cored tube prepared by the present invention has uniform zirconium distribution and low burning rate.
[0030] In summary, the present invention strictly controls various processes from material selection to preparation, and through filling and drawing, the obtained copper-zirconium intermediate alloy tube is a seamless copper tube with few impurities, dense and uniform, no air residue, and low melting point; at the same time, the flow trough temperature of the non-vacuum smelting copper-chromium-zirconium alloy and the wire feeding speed of the copper-zirconium intermediate alloy core tube are controlled, so that the oxidation and loss of zirconium can be reduced, the distribution is uniform, and the molded production can be realized.
[0031] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A copper-zirconium master alloy cored tube, characterized in that: It comprises an inner core and a cladding, wherein the cladding is a T2 copper tube, and the inner core is copper-zirconium intermediate alloy particles, the particle size of which is ≤1.0 mm and does not contain unalloyed or insufficiently alloyed elements.
2. The copper-zirconium master alloy cored tube according to claim 1, characterized in that: The zirconium content in the copper-zirconium master alloy particles is 45-55%.
3. A method for preparing a copper-zirconium master alloy cored tube according to any one of claims 1 to 2, characterized in that: The following steps are involved: (1) Prepare T2 copper tube and copper-zirconium master alloy for standby use, wherein the weight ratio of the two is 0.35-1; (2) Crushing and screening: The purchased copper-zirconium master alloy is crushed and screened by a jaw crusher to separate and remove large particles that are not fully alloyed, and to screen out master alloy particles with a particle size of ≤1.0 mm; (3) Particle loading: The master alloy particles obtained in step (2) are loaded into a T2 copper tube, and the air in the tube is expelled by vibration; (4) Disc drawing: the copper tube filled with copper-zirconium master alloy particles in step (3) is placed in a disc and drawn in multiple passes; (5) Annealing: The copper tube drawn in step (4) is annealed under nitrogen protection to obtain a copper-zirconium master alloy core tube.
4. The preparation method according to claim 3, characterized in that: In step (1), the ratio of the outer diameter to the wall thickness of the T2 copper tube is between 10 and 28.
5. The preparation method according to claim 3, characterized in that: In step (4), the diameter reduction rate of the copper tube after drawing is 30-80%, and the single-pass diameter reduction rate is ≤20%.
6. The preparation method according to claim 3, characterized in that: In step (5), the annealing temperature is 350-550°C.
7. An application of the copper-zirconium master alloy cored tube as claimed in any one of claims 1 to 2 or the copper-zirconium master alloy cored tube prepared by the preparation method as claimed in any one of claims 3 to 6 in non-vacuum melting and casting of copper-chromium-zirconium alloy large flat ingots, characterized in that: The application method is as follows: S1. Copper smelting: Use coreless induction furnace to melt electrolytic copper plate. The melting process is completely covered with charcoal to prevent air from entering the copper liquid. The melting temperature is 1100-1200℃; S2. Argon degassing: After heating the molten copper to 1150-1200℃, let it stand for 5-15min, and introduce compressed argon gas to the bottom of the copper liquid through a graphite tube for 5-15min. The charcoal should be fully covered during the whole process. S3. Adding copper-chromium master alloy: After degassing, the temperature of the molten copper is raised to 1200-1250°C, and the copper-chromium master alloy is added according to the alloy composition ratio to fully melt the master alloy, and the temperature is maintained at 1200-1250°C, and the charcoal is fully covered; S4. Pour the molten copper: When the temperature of the molten copper reaches 1200-1250°C, open the graphite stopper rod, and the molten copper enters the launder equipped with an induction coil, and the launder induction coil heats the molten copper at high power; S5. Adding copper-zirconium master alloy cored tube: During the process of copper liquid filling the launder, start the wire feeder and add the copper-zirconium master alloy cored tube at a certain speed. The wire feeder speed is determined by the alloy composition ratio; S6. Casting: When the copper liquid fills 50-85% of the flow channel volume, the graphite stopper of the flow channel is opened, and the copper liquid enters the crystallizer for casting. At the same time, the copper liquid in the crystallizer is completely covered with carbon black powder to obtain an ingot.
8. The use according to claim 7, characterized in that: In S4, the induction coil is installed in the middle part of the flow channel, and the heating power during production is 0-30kW; before the copper liquid flows in, the flow channel is heated and baked with burning charcoal for 30-40 minutes in advance; the induction coil is baked with a low current.
9. The use according to claim 7, characterized in that: In S5, the wire feeder adopts PLC to control the speed and is linked to the speed of the ingot casting machine; the wire feeding speed of the wire feeder is controlled according to the amount of Zr element 0.15% in the ingot produced per unit time.
10. The use according to claim 7, characterized in that: In S6, the casting speed is 50-100 mm / min.
Citation Information
Patent Citations
All-copper core spun yarn friction plate
CN104632962A
Preparation method of copper-chromium-zirconium alloy wire
CN110218898A
Core-spun yarn for manufacturing copper-chromium-zirconium alloy and preparation method and application of core-spun yarn
CN115198134A
Method for production of a fuel casing tube for a nuclear reactor and tube obtained thus
CN1993489A
Copper alloy wire for connector and method for manufacture thereof
WO2021148054A1