A corrosion inhibitor composition, preparation method and application thereof

By introducing a combination of the first corrosion inhibitor and the second corrosion inhibitor into the corrosion inhibitor in the oil field, combining vitamin E, bisphenol A and nonionic surfactant to optimize the molecular structure, the existing corrosion inhibitors are solved in complex oil fields. The problems of adsorption force and stability in the environment improve the corrosion inhibition effect and equipment life.

CN118835251BActive Publication Date: 2024-12-03SICHUAN SHANG ZHI DENG NEW MATERIALS CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411321563.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

During the oil field mining process, existing adsorption corrosion inhibitors are prone to rupture or peeling of corrosion inhibitors due to complex fluid output and unstable flow conditions, reducing adsorption protection effect, and complex molecular structure leads to complex preparation process and high cost. Impact solubility and corrosion inhibition effect.

Method used

A corrosion inhibitor composition is adopted, including a first corrosion inhibitor (containing a long carbon alkenyl group, an imidazole ring, a thiophene ring and a bisamide bond) and a second corrosion inhibitor (2-mercaptobenzimidazole), combined with vitamin E, bisphenol A and nonionic surfactants improve adsorption force and stability by optimizing molecular structure and combination use.

Benefits of technology

It achieves the formation of a stable adsorption layer on the metal surface, reduces corrosion rate, improves corrosion inhibition effect and stability, is suitable for high sulfur-containing multi-phase flow oil well environment, reduces the dissolution and loss of corrosion inhibitors, and extends the service life of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835251B_ABST
    Figure CN118835251B_ABST
Patent Text Reader

Abstract

The present invention provides a corrosion inhibitor composition, a preparation method and application thereof, belonging to the technical field of oil and gas field development; a first corrosion inhibitor is synthesized by carboxyethyl imidazoline and 2-thiophene carboxylic acid hydrazide, the first corrosion inhibitor is closely connected by an imidazole ring, a thiophene ring and a diamide bond, and can be firmly adsorbed on a metal surface under a small steric hindrance, combined with the excellent hydrophobicity possessed by the alkenyl group of a long carbon chain, the first corrosion inhibitor is used in the exploitation and gathering of oil and water wells, and can show good corrosion inhibition performance. Further, the first corrosion inhibitor, together with a second corrosion inhibitor, vitamin E, bisphenol A, etc., can further improve the corrosion inhibition performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil and gas field development, and specifically relates to a corrosion inhibitor composition, a preparation method and application thereof. Background Art

[0002] In the process of oil and gas field development, corrosion inhibitors play an indispensable role. They are crucial to protecting oil field mining and gathering and transportation equipment from corrosion and extending the service life of equipment. At present, most of the oil field corrosion inhibitors used at home and abroad are adsorption-type corrosion inhibitors, and their main corrosion inhibition components are organic matter, such as chain organic amines and their derivatives, imidazolines and their salts, quaternary ammonium salts, rosin derivatives, sulfonates, iminoacetic acid derivatives and acetylenic alcohols. These corrosion inhibitors work by forming a dense protective film on the metal surface to isolate the corrosive medium, and their corrosion inhibition efficiency is closely related to their adsorption strength on the metal surface.

[0003] However, in the actual oilfield exploitation process, the complexity of the output has challenged the performance of these adsorption-type corrosion inhibitors. The fluid produced by the oilfield usually contains corrosive gases such as hydrogen sulfide and carbon dioxide, as well as impurities such as solid particles. The complexity of these components can easily lead to the rupture or peeling of the corrosion inhibition film, thereby reducing its adsorption protection effect; in addition, the fluid produced by the oilfield is very unstable when flowing (especially when multiphase flow such as gas and liquid exists at the same time), and the pressure fluctuations and flow rate changes inside the pipeline will affect the stability and integrity of the corrosion inhibition film. Changes in these conditions can easily reduce the adsorption effect of the corrosion inhibitor on the metal surface, and even cause the corrosion inhibitor to dissolve or lose, thereby accelerating the corrosion of the metal.

[0004] Based on this, the oilfield industry needs to continuously explore and develop corrosion inhibitors with stronger adsorption, higher stability and better adaptability. Chinese patent ZL202011558040.X discloses an oil-soluble high-efficiency imidazoline corrosion inhibitor with multiple adsorption sites and its preparation method. The introduction of three imidazoline rings in the molecular structure of the imidazoline corrosion inhibitor effectively improves the adsorption capacity of the corrosion inhibitor on the metal matrix, and the three 17-carbon chains improve the hydrophobicity of the corrosion inhibitor and further improve the corrosion inhibition ability of the corrosion inhibitor. However, there are still many problems with the above-mentioned oil-soluble and efficient imidazoline corrosion inhibitor with multiple adsorption sites: first, its molecular structure is complex, containing three imidazole rings, multiple ethylamine groups and three heptadecanyl groups, which makes it easy to produce large steric hindrance on the metal surface. This steric hindrance will hinder the sufficient contact between the compound molecules and the metal surface, thereby reducing the adsorption efficiency; secondly, due to the complex molecular structure of the corrosion inhibitor, a variety of substances need to be introduced during its preparation, resulting in a complex preparation process and high cost; in addition, its molecular structure is large and contains a large number of carbon atoms, and there are also many branched structures, which will affect its solubility, and therefore its corrosion inhibition effect is affected.

[0005] In view of this, it is necessary to further improve the existing technology and develop corrosion inhibitors or their compositions with better stability and stronger adsorption capacity. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a corrosion inhibitor composition, a preparation method and application thereof, with the aim of solving at least one of the above problems.

[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0008] A corrosion inhibitor composition comprises the following raw material components by weight: 15-20 parts of a first corrosion inhibitor, 3-5 parts of a second corrosion inhibitor, 0.1-0.3 parts of vitamin E, 1.0-1.5 parts of bisphenol A, 40-60 parts of an organic solvent and 2-3 parts of a nonionic surfactant; wherein the structural formula of the first corrosion inhibitor is:

[0009] ,

[0010] In the formula, R is C 10 -C 20 The alkenyl group;

[0011] The second corrosion inhibitor is 2-mercaptobenzimidazole.

[0012] Preferably, R is heptadecenyl.

[0013] Preferably, the raw material components of the corrosion inhibitor composition further include 0.2 to 0.4 parts by weight of nano titanium dioxide.

[0014] Compared with the prior art, the present invention has at least the following beneficial effects:

[0015] 1. The first corrosion inhibitor prepared by the present invention comprises a long carbon chain alkenyl group (R), an imidazole ring, a thiophene ring and a double amide bond connected between the imidazole ring and the thiophene ring. The long carbon chain alkenyl group (R) ensures that the molecule has excellent hydrophobicity, which is essential for forming a stable adsorption layer on the metal surface because it can effectively isolate the corrosive medium and reduce the corrosion rate of the metal; the introduction of the imidazole ring and the thiophene ring not only enhances the chemical stability and thermal stability of the molecule, but also provides additional coordination sites, so that the corrosion inhibitor can form a stronger chemical bond with the metal surface, thereby improving the corrosion inhibition effect; the presence of the double amide bond further enhances The rigidity and planarity of the molecule are enhanced, which helps to evenly distribute the molecule on the metal surface and improve the corrosion inhibition efficiency; the imidazole ring, thiophene ring and diamide bond are tightly connected, with little steric hindrance. This structural design makes the adsorption of the entire molecule on the metal surface more stable. The structure connected by the above three tends to maintain planarity, which can ensure sufficient coverage on the metal surface and help stacking between molecules, thereby improving the slow-release effect. The olefin end of the long carbon chain can be dissolved in oil, while the end where the above three are located can be firmly adsorbed on the metal surface. This structure enables the corrosion inhibitor to show good performance in both oil and water environments;

[0016] 2. The first corrosion inhibitor and the second corrosion inhibitor are introduced into the composition at the same time, and the two act synergistically to further improve the slow-release effect; in addition, the first corrosion inhibitor, the second corrosion inhibitor, vitamin E, bisphenol A and non-ionic surfactant are combined to achieve a better corrosion inhibition effect. This product is suitable for use in high-sulfur multiphase flow oil wells with low water content. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:

[0018] Figure 1 It is a schematic diagram of the reaction equation for preparing the first corrosion inhibitor intermediate of the present invention;

[0019] Figure 2 It is a schematic diagram of a reaction equation for preparing a first corrosion inhibitor through a first corrosion inhibitor intermediate according to the present invention;

[0020] Figure 3 It is a schematic diagram of the principle of the test system for performing corrosion test of the present invention;

[0021] Among them, 1-high pressure tank, 2-recovery tank, 3-test pipeline, 4-flow regulating valve, 5-liquid flow meter, 6-first one-way valve, 7-hanging plate test area, 8-second one-way valve, 9-gas injection pipeline. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The illustrative embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0023] The present invention provides a corrosion inhibitor composition, which comprises the following raw material components by weight: 15-20 parts of a first corrosion inhibitor, 3-5 parts of a second corrosion inhibitor, 0.1-0.3 parts of vitamin E, 1.0-1.5 parts of bisphenol A, 40-60 parts of an organic solvent and 2-3 parts of a nonionic surfactant;

[0024] Wherein, the structural formula of the first corrosion inhibitor is:

[0025] ,

[0026] In the formula, R is C 10 -C 20 for example, heptadecenyl;

[0027] The second corrosion inhibitor is 2-mercaptobenzimidazole.

[0028] Preferably, the organic solvent is white oil or mineral oil, and the nonionic surfactant is castor oil polyoxyethylene ether type nonionic surfactant, for example, castor oil polyoxyethylene ether EL-40, EL-60 and the like.

[0029] In a further preferred embodiment, the raw material components of the corrosion inhibitor composition further include 0.2 to 0.4 parts by weight of nano titanium dioxide.

[0030] Taking R as a 17-carbon alkenyl group as an example, the first corrosion inhibitor is prepared by the following method, which includes the following steps:

[0031] S1. Dissolve 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole in DMSO (dimethyl sulfoxide) solvent at room temperature (preferably 25°C) to form a 0.2-0.5M solution;

[0032] Among them, 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole is a carboxyethyl imidazoline of model RX-403 purchased from Shaanxi Rixin Petrochemical Co., Ltd., and its chemical structure is as follows:

[0033] ;

[0034] S2. Add 1.2-1.5 molar equivalents of EDC [1-ethyl-3-(3-dimethylaminopropyl) carbodiimide] relative to 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole and 1.1-1.2 molar equivalents of NHS (N-hydroxysuccinimide) relative to EDC to the above solution to react and form an active ester intermediate (see Figure 1 ); During this process, the reaction progress is regularly monitored using techniques such as TLC (thin layer chromatography) or HPLC (high performance liquid chromatography) to determine whether the activation is complete;

[0035] S3. Remove unreacted EDC and NHS by dialysis, extraction or the like, and then dry and remove the solvent under vacuum (for example, evaporate the solvent by a rotary evaporator) to obtain a dry active ester intermediate; dialysis, vacuum drying or the like is mainly for purifying the active ester intermediate, ensuring the stability and reactivity of the active ester intermediate in subsequent reactions, and reducing the possibility of side reactions;

[0036] S4. In an ice water bath at 0°C, the dried active ester intermediate is redissolved in DMSO and stirred to form a uniform active ester intermediate solution (the amount of DMSO added is preferably such that the active ester intermediate is completely dissolved);

[0037] S5. Add 2-thiophenecarboxylic acid hydrazide in an amount equimolar to 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole to the active ester intermediate solution at 0°C and stir evenly. While adding 2-thiophenecarboxylic acid hydrazide and stirring, add 0.05-0.2 molar equivalent of Et3N (triethylamine) relative to 2-thiophenecarboxylic acid hydrazide to the active ester intermediate solution according to the amount of 2-thiophenecarboxylic acid hydrazide added. Then, maintain the temperature at 0°C and stir at a constant speed for 6 to 8 hours to ensure sufficient mixing and reaction (during which periodic sampling is performed and the reaction progress is monitored by TLC, HPLC, etc. to ensure complete conversion). After the reaction is completed, a mixed solution containing the first corrosion inhibitor is obtained (see Figure 2 );

[0038] In step S5, a small amount of Et3N is added while adding 2-thiophenecarboxylic acid hydrazide. The introduced Et3N can effectively accelerate the reaction process and ensure the formation of the target product. Due to the influence of factors such as steric hindrance, the addition of Et3N can preferentially act on the amino group at the end of 2-thiophenecarboxylic acid hydrazide, which forms an ion pair by accepting protons, enhances the nucleophilicity of the amino group at the end of 2-thiophenecarboxylic acid hydrazide, and promotes its reaction with the active ester intermediate. In addition, in this process, triethylamine can also participate in the formation of temporary intermediates, stabilize the transition state of the reaction, reduce the activation energy of the reaction, and thus accelerate the reaction. It should be noted that in this step, the amount of Et3N needs to be strictly controlled. If the amount of Et3N is too much, another amino group in 2-thiophenecarboxylic acid hydrazide except the end amino group may also be activated, resulting in the production of by-products; if the amount of Et3N is too little, a longer reaction time is required, and under a longer reaction time, a lot of by-products will also be produced;

[0039] S6. The mixed solution containing the first corrosion inhibitor is subjected to extraction, drying, separation, and other treatments to obtain a first corrosion inhibitor of high purity. Exemplarily, a sufficient amount of an organic solvent (such as dichloromethane or chloroform) that is incompatible with DMSO is added to the mixed solution containing the first corrosion inhibitor for liquid-liquid extraction to separate the organic phase containing the first corrosion inhibitor, and then the separated organic phase is dried by anhydrous magnesium sulfate or anhydrous sodium sulfate to remove possible residual moisture and DMSO, and then the solid desiccant such as anhydrous magnesium sulfate or anhydrous sodium sulfate is separated from the organic phase by filtration or centrifugation; the separated organic phase is subjected to a rotary evaporator or a reduced pressure distillation to remove the organic solvent that is incompatible with DMSO used in the above-mentioned liquid-liquid extraction process to obtain a crude product of the first corrosion inhibitor, and the crude product is further purified, such as by column chromatography, crystallization or recrystallization, to obtain a first corrosion inhibitor of high purity.

[0040] The technical scheme of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. In the following examples and comparative examples, R in the first corrosion inhibitor is a 17-carbon alkenyl group, and the structural formula of the first corrosion inhibitor is:

[0041] ;

[0042] The second corrosion inhibitor is 2-mercaptobenzimidazole, the organic solvent is white oil, and the non-ionic surfactant is castor oil polyoxyethylene ether EL-40, which will not be described in detail below.

[0043] Embodiment 1

[0044] A corrosion inhibitor composition comprises the following raw material components by weight: 15 parts of a first corrosion inhibitor, 3 parts of a second corrosion inhibitor, 0.1 parts of vitamin E, 1.0 parts of bisphenol A, 40 parts of an organic solvent and 2 parts of a nonionic surfactant.

[0045] The preparation method of the corrosion inhibitor composition is as follows: in a nitrogen environment, an organic solvent is heated to 60°C, then, while maintaining a constant temperature of 60°C, weighed non-ionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then the first corrosion inhibitor and the second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, while stirring, the mixture is cooled to room temperature (about 25°C).

[0046] Embodiment 2

[0047] A corrosion inhibitor composition comprises the following raw material components by weight: 18 parts of a first corrosion inhibitor, 3 parts of a second corrosion inhibitor, 0.1 parts of vitamin E, 1.0 parts of bisphenol A, 40 parts of an organic solvent and 2 parts of a nonionic surfactant.

[0048] The preparation method of the corrosion inhibitor composition is as follows: in a nitrogen environment, an organic solvent is heated to 60°C, then, while maintaining a constant temperature of 60°C, weighed non-ionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then the first corrosion inhibitor and the second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, while stirring, the mixture is cooled to room temperature (about 25°C).

[0049] Embodiment 3

[0050] A corrosion inhibitor composition comprises the following raw material components by weight: 20 parts of a first corrosion inhibitor, 3 parts of a second corrosion inhibitor, 0.1 parts of vitamin E, 1.0 parts of bisphenol A, 40 parts of an organic solvent and 2 parts of a nonionic surfactant.

[0051] The preparation method of the corrosion inhibitor composition is as follows: in a nitrogen environment, an organic solvent is heated to 60°C, then, while maintaining a constant temperature of 60°C, weighed non-ionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then the first corrosion inhibitor and the second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, while stirring, the mixture is cooled to room temperature (about 25°C).

[0052] Embodiment 4

[0053] A corrosion inhibitor composition comprises the following raw material components by weight: 20 parts of a first corrosion inhibitor, 5 parts of a second corrosion inhibitor, 0.3 parts of vitamin E, 1.5 parts of bisphenol A, 60 parts of an organic solvent and 3 parts of a nonionic surfactant.

[0054] The preparation method of the corrosion inhibitor composition is as follows: in a nitrogen environment, an organic solvent is heated to 60°C, then, while maintaining a constant temperature of 60°C, weighed non-ionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then the first corrosion inhibitor and the second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, while stirring, the mixture is cooled to room temperature (about 25°C).

[0055] Embodiment 5

[0056] A corrosion inhibitor composition comprises the following raw material components by weight: 15 parts of a first corrosion inhibitor, 3 parts of a second corrosion inhibitor, 0.1 parts of vitamin E, 1.0 parts of bisphenol A, 40 parts of an organic solvent, 2 parts of a nonionic surfactant and 0.2 parts of nano titanium dioxide.

[0057] The preparation method of the corrosion inhibitor composition is as follows: in a nitrogen environment, an organic solvent is heated to 60°C, then, while maintaining a constant temperature of 60°C, weighed non-ionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then nano titanium dioxide, a first corrosion inhibitor and a second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, while stirring, the mixture is cooled to room temperature (about 25°C).

[0058] Embodiment 6

[0059] A corrosion inhibitor composition comprises the following raw material components by weight: 15 parts of a first corrosion inhibitor, 3 parts of a second corrosion inhibitor, 0.1 parts of vitamin E, 1.0 parts of bisphenol A, 40 parts of an organic solvent, 2 parts of a nonionic surfactant and 0.3 parts of nano titanium dioxide.

[0060] The preparation method of the corrosion inhibitor composition is as follows: in a nitrogen environment, an organic solvent is heated to 60°C, then, while maintaining a constant temperature of 60°C, weighed non-ionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then nano titanium dioxide, a first corrosion inhibitor and a second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, while stirring, the mixture is cooled to room temperature (about 25°C).

[0061] Embodiment 7

[0062] A corrosion inhibitor composition comprises the following raw material components by weight: 15 parts of a first corrosion inhibitor, 3 parts of a second corrosion inhibitor, 0.1 parts of vitamin E, 1.0 parts of bisphenol A, 40 parts of an organic solvent, 2 parts of a nonionic surfactant and 0.4 parts of nano titanium dioxide.

[0063] The preparation method of the corrosion inhibitor composition is as follows: in a nitrogen environment, an organic solvent is heated to 60°C, then, while maintaining a constant temperature of 60°C, weighed non-ionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then nano titanium dioxide, a first corrosion inhibitor and a second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, while stirring, the mixture is cooled to room temperature (about 25°C).

[0064] Embodiment 8

[0065] A corrosion inhibitor composition comprises the following raw material components by weight: 20 parts of a first corrosion inhibitor, 5 parts of a second corrosion inhibitor, 0.3 parts of vitamin E, 1.5 parts of bisphenol A, 60 parts of an organic solvent, 3 parts of a nonionic surfactant and 0.4 parts of nano titanium dioxide.

[0066] The preparation method of the corrosion inhibitor composition is as follows: in a nitrogen environment, an organic solvent is heated to 60°C, then, while maintaining a constant temperature of 60°C, weighed non-ionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then nano titanium dioxide, a first corrosion inhibitor and a second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, while stirring, the mixture is cooled to room temperature (about 25°C).

[0067] Comparative Example 1

[0068] The difference between the corrosion inhibitor composition of Comparative Example 1 and Example 1 is that the first corrosion inhibitor is not added in Comparative Example 1, but the first corrosion inhibitor in Example 1 is replaced by an equal mass portion of the second corrosion inhibitor (that is, the mass portion of the second corrosion inhibitor in Comparative Example 1 is 15+3=18 parts). Except for the above differences, the remaining components and the corresponding preparation method are the same as those in Example 1.

[0069] Comparative Example 2

[0070] The difference between the corrosion inhibitor composition of Comparative Example 2 and Example 1 is that the second corrosion inhibitor is not added in Comparative Example 2, but the second corrosion inhibitor in Example 1 is replaced by an equal mass portion of the first corrosion inhibitor (that is, the mass portion of the first corrosion inhibitor in Comparative Example 2 is 15+3=18 parts). Except for the above differences, the remaining components and the corresponding preparation method are the same as those in Example 1.

[0071] Comparative Example 3

[0072] The difference between the corrosion inhibitor composition of Comparative Example 3 and Example 1 is that in Comparative Example 3, the first corrosion inhibitor in Example 1 is replaced by an equal mass portion of 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole. Except for the above differences, the remaining components and the corresponding preparation method are the same as those in Example 1.

[0073] Comparative Example 4

[0074] The difference between the corrosion inhibitor composition of Comparative Example 4 and Example 1 is that vitamin E, bisphenol A and nonionic surfactant are not added in Comparative Example 4. Except for the above differences, the remaining components and the corresponding preparation method are the same as those of Example 1.

[0075] Performance Test:

[0076] use Figure 3The test system shown in the figure performs corrosion test, and the test system includes a high-pressure tank 1, a recovery tank 2 and a test pipeline 3, wherein the test pipeline 3 connects the high-pressure tank 1 and the recovery tank 2, and a flow regulating valve 4, a liquid flow meter 5, a first one-way valve 6 and a second one-way valve 8 are sequentially arranged on the test pipeline 3 along the direction from the high-pressure tank 1 to the recovery tank 2, and the first one-way valve 6 and the second one-way valve 8 can only allow the fluid to flow from the high-pressure tank 1 to the recovery tank 2, and a coupon test area 7 is formed on the test pipeline 3 between the first one-way valve 6 and the second one-way valve 8, and a gas injection pipeline 9 is also arranged between the coupon test area 7 and the first one-way valve 6, and the diameter of the gas injection pipeline 9 is equal to the diameter of the test pipeline 3. Among them, the flow regulating valve 4 is associated with the liquid flow meter 5, and is used to realize the flow regulation of the liquid from the high-pressure tank 1 (for example, the opening of the flow regulating valve 4 is feedback-regulated by the detected liquid flow, so as to keep the liquid flow constant within the required flow range). Furthermore, a switch valve and a gas flow meter (not shown in the figure) are also provided on the gas injection pipeline 9 to adjust the flow of the injected gas. The switch valve is provided near the test pipeline 3, and the gas flow meter is located on the side of the switch valve away from the test pipeline 3; a temperature regulating mechanism (not shown in the figure) is provided at the high-pressure tank 1 to regulate the temperature of the liquid therein. The recovery tank 2 is a low-pressure tank, and its rear end can also be connected to exhaust gas treatment equipment, etc. Furthermore, a circulation pipeline is also connected between the high-pressure tank 1 and the recovery tank 2 to circulate the liquid used in the same test (returning to the high-pressure tank 1 after pressurization) to reduce the consumption of oil products in the experiment (the above is the main scheme of the test system, and its details are not repeated). By adopting the above test system, the gathering and transportation situation of the oil and gas field site can be more realistically reflected. The high-pressure tank 1 can simulate a stable well site fluid production source, and the test pipeline 3 is used to simulate the gathering and transportation pipeline. Since the fluid actually produced on site is often a multiphase mixed fluid containing oil, gas and water, and this multiphase fluid is not easy to simulate in the laboratory, a gas injection pipeline 9 is set up, which is closer to the actual situation of gas-liquid fluctuations in the oil and gas gathering and transportation process.

[0077] Specifically, in the corrosion test of this embodiment, the liquid contained in the high-pressure tank 1 is an oil-water mixed fluid collected from an oil and gas well in the tower. The water content is about 13% after centrifugal separation, the chloride ion concentration of the water is about 112000 mg / L after chloride ion determination, and the hydrogen sulfide content is about 1500 mg / m by iodine titration. 3; The material to be corroded used in the test is ‌L360NCS pipeline steel, which is made into a sample hanger with a size of 30mm×20mm×5mm. Before the test, it is polished, cleaned and dried, and placed in the hanger test area 7 of the test pipeline 3 after weighing and measuring the size. Before the test starts, the liquid in the high-pressure tank 1 is heated to 50°C and maintained constant by the temperature regulating mechanism, the pressure of the high-pressure tank 1 is adjusted to 20MPa, and then 1000ppm (mass concentration) of the corrosion inhibitor composition is added to the liquid in the high-pressure tank 1 and stirred evenly. Since there is a relationship between flow rate and flow velocity, the formula Q=v*A, where Q is the flow rate, v is the flow velocity, A is the corresponding inner diameter of the pipeline, and A is a fixed and known parameter, the fluid can be limited to flow at the desired flow rate by adjusting the flow rate.

[0078] In this embodiment, the corrosion test is carried out in two parts, namely, only the liquid test part and the gas-liquid mixed test part. In the liquid test part, the corrosion conditions of the liquid at flow rates of 6m / s, 8m / s, 10m / s, 12m / s and 16m / s are tested respectively (reflected by the average corrosion rate). In the gas-liquid mixed test part, while injecting liquid into the coupon test area 7, gas with the same flow rate (since the diameter of the gas injection pipeline 9 is equal to the diameter of the test pipeline 3, the same flow rate is essentially the same flow rate) is injected. The flow rate is tested in the manner of 3m / s+3m / s (i.e., the liquid injection speed is 3m / s, and the gas injection speed is also 3m / s), 5m / s+5m / s and 8m / s+8m / s. The flow rate is controlled by the corresponding flow meter and valve. Each corrosion test time is 72h, and the sample coupon needs to be replaced for each corrosion test. In order to save test time, 12 sets of the same test systems are used for simultaneous testing. Each set of test systems corresponds to a corrosion inhibitor composition. For example, the corrosion inhibitor composition of Example 1 uses a set of test systems to test its corrosion at different flow rates. The corrosion inhibitor composition of Example 2 uses another set of test systems, and so on. It should be noted that during the flow of fluid, the corrosion resistance of the adsorption-type corrosion inhibitor is closely related to the flow rate. The increase in flow rate will enhance the scouring shear force of the fluid, thereby affecting its corrosion resistance. Therefore, the corrosion resistance at different flow rates can reflect the adsorption strength and stability of the corrosion inhibitor.

[0079] In this embodiment, corrosion tests are performed for different flow rates, and the specific test results are as follows:

[0080]

[0081] As can be seen from the above table, at the same flow rate, the average corrosion rate of comparative examples 1 to 4 is much higher than that of all embodiments of the present invention, indicating that embodiments 1 to 8 have better corrosion inhibition effects than comparative examples 1 to 4. Compared with embodiment 1, comparative examples 1 and 2 lack the first corrosion inhibitor and the second corrosion inhibitor, respectively, that is, only one of the first corrosion inhibitor and the second corrosion inhibitor is used for corrosion inhibition. In this case, the corrosion effect is much lower than that of embodiment 1 (under the same mass fraction) in which the first corrosion inhibitor and the second corrosion inhibitor are used in combination, indicating that the first corrosion inhibitor and the second corrosion inhibitor produce a synergistic effect and improve the corrosion inhibition effect when combined. Further, referring to the above table, at the same flow rate, the average corrosion rate of comparative example 2 is lower than that of comparative example 1, indicating that the first corrosion inhibitor prepared by the present invention has better corrosion inhibition performance than the second corrosion inhibitor when used alone. Since the corrosion inhibition test is carried out by flow rate, it reflects from the side that the first corrosion inhibitor has stronger adsorption and stability under the flushing shear force of the fluid, which may be caused by its own specific molecular structure. The first corrosion inhibitor includes a long carbon chain alkenyl group (R), an imidazole ring, a thiophene ring and a diamide bond connecting the imidazole ring and the thiophene ring. The long carbon chain alkenyl group (R) ensures that the molecule has excellent hydrophobicity, which helps it dissolve in oil and forms an effective isolation from the corrosive medium. The introduction of the imidazole ring and the thiophene ring not only enhances the chemical stability and thermal stability of the molecule, but also provides additional coordination sites, so that the corrosion inhibitor can form a stronger chemical bond with the metal surface, thereby improving the corrosion inhibition effect; the presence of the diamide bond further enhances the rigidity and planarity of the molecule, which helps the uniform distribution of the molecule on the metal surface and improves the corrosion inhibition efficiency; the imidazole ring, the thiophene ring and the diamide bond further enhance the rigidity and planarity of the molecule, which helps the uniform distribution of the molecule on the metal surface and improves the corrosion inhibition efficiency. The ring and the diamide bond form a multi-point connection and the three are tightly connected, with small steric hindrance. This structural design makes the adsorption of the entire molecule on the metal surface more stable, which helps to form a large and stable corrosion inhibition film on the metal surface. The structure of the three connections tends to maintain planarity, which can ensure that it has sufficient coverage on the metal surface, helps to stack between molecules, and thus improves the sustained release effect. In short, the first corrosion inhibitor in the present invention is dissolved in the oil at one end through the long carbon chain olefin group, and the other end is firmly adsorbed on the metal surface through densely adjacent multi-point positions, thereby ensuring sufficient adsorption force on the metal surface, thereby ensuring that it has sufficient corrosion inhibition ability at high flow rates.

[0082] Further, referring to Comparative Example 3 in the above table, when the first corrosion inhibitor in Example 1 is replaced with an equal mass portion of 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole, its corrosion inhibition performance is significantly reduced. This may be because 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole contains a carboxyl group, which makes the substance easily soluble in water and its solubility in oil is greatly reduced. Further referring to Comparative Example 4 in the above table, when auxiliary ingredients such as vitamin E, bisphenol A and non-ionic surfactant are not added, the corrosion inhibition performance of the composition also decreases significantly (compared with Example 1), indicating that the above auxiliary ingredients can promote the corrosion inhibition performance of the first corrosion inhibitor and the second corrosion inhibitor, thereby improving their corrosion inhibition performance. In Comparative Example 4, since the combination of the first corrosion inhibitor and the second corrosion inhibitor is still used, its average corrosion rate at each flow rate is lower than the corresponding average corrosion rate of Comparative Examples 1 and 2, once again proving that the first corrosion inhibitor and the second corrosion inhibitor produce a synergistic effect and improve the corrosion inhibition effect when combined, and the combination of the two components can improve its corrosion resistance in the oil field gathering and transportation process. In addition, a certain amount of nano-titanium dioxide is added to Examples 5 to 8. Under low flow rate conditions (for example, when only liquid is present, <10 m / s), the average corrosion rate is significantly reduced. When the flow rate increases, the average corrosion rate is basically the same as when no addition is made, indicating that adding a certain amount of nano-titanium dioxide helps to improve the corrosion resistance of the material under low flow rate, which is very beneficial for oil wells, especially oil wells with less gas content, to collect and transport produced fluids, because under normal circumstances, the flow rate of the fluid produced by the oil well will not exceed 10 m / s during collection and transportation (the reason why the minimum speed used in the test is also 6 m / s is that a greater degree of corrosion can occur under high-speed conditions, and corrosion testing can be achieved in a shorter time to ensure the accuracy of the test data). In addition, under the gas-liquid mixed test, the test results are basically consistent with those under liquid conditions only, and will not be repeated here. In general, the present invention provides an oil-soluble corrosion inhibitor composition suitable for use in an environment where oil, gas and water coexist, especially in a high-sulfur oil well with low water content.

[0083] Finally, it should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0084] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to the embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A corrosion inhibitor composition, characterized in that It at least contains a first corrosion inhibitor, wherein the structural formula of the first corrosion inhibitor is: , In the formula, R is C 10 -C 20 The alkenyl group.

2. A corrosion inhibitor composition according to claim 1, characterized in that: The invention comprises the following raw material components by weight: 15 to 20 parts of a first corrosion inhibitor, 3 to 5 parts of a second corrosion inhibitor, 0.1 to 0.3 parts of vitamin E, 1.0 to 1.5 parts of bisphenol A, 40 to 60 parts of an organic solvent and 2 to 3 parts of a non-ionic surfactant; wherein the second corrosion inhibitor is 2-mercaptobenzimidazole.

3. A corrosion inhibitor composition according to claim 1 or 2, characterized in that: R is a heptadeca-alkenyl group.

4. A corrosion inhibitor composition as claimed in claim 2, characterized in that: The corrosion inhibitor composition further comprises 0.2 to 0.4 parts by weight of nano titanium dioxide.

5. A corrosion inhibitor composition as claimed in claim 4, characterized in that: By weight, the corrosion inhibitor composition contains 0.3 parts of nano titanium dioxide.

6. A method for preparing a corrosion inhibitor composition, the method being used for preparing the corrosion inhibitor composition according to any one of claims 1 to 3, characterized in that: It includes the following steps: In a nitrogen environment, the organic solvent is heated to 60° C., then, while maintaining a constant temperature of 60° C., weighed nonionic surfactant, vitamin E and bisphenol A are added in sequence while stirring, and stirred until completely dissolved, and then the first corrosion inhibitor and the second corrosion inhibitor are added in sequence, and stirring is continued for 30 minutes to ensure uniform dispersion, and then, the mixture is cooled to room temperature while stirring to obtain; Alternatively, the preparation method is used to prepare the corrosion inhibitor composition described in any one of claims 4-5, which comprises the following steps: heating the organic solvent to 60°C under a nitrogen environment, then, maintaining the constant temperature at 60°C, adding weighed non-ionic surfactant, vitamin E and bisphenol A in sequence while stirring, stirring until completely dissolved, then adding nano titanium dioxide, the first corrosion inhibitor and the second corrosion inhibitor in sequence, stirring continuously for 30 minutes to ensure uniform dispersion, and then cooling to room temperature while stirring.

7. The method for preparing a corrosion inhibitor composition according to claim 6, wherein: R is a 17-carbon alkenyl group; characterized in that the first corrosion inhibitor is prepared by the following steps: S1. Dissolve 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole in DMSO solvent at room temperature to form a 0.2-0.5 M solution; Among them, the chemical structural formula of 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole is: , S2, adding 1.2-1.5 molar equivalents of EDC relative to 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole and 1.1-1.2 molar equivalents of NHS relative to EDC to the above solution to react and form an active ester intermediate; S3, removing unreacted EDC and NHS, and then drying to remove the solvent under vacuum to obtain a dry active ester intermediate; S4. Redissolve the dried active ester intermediate in DMSO in an ice water bath at 0°C and stir to form a uniform active ester intermediate solution; S5, adding 2-thiophenecarboxylic acid hydrazide in an amount equimolar to 1-(2-carboxyethyl)-2-(heptadecenyl)-imidazole to the active ester intermediate solution at 0°C and stirring evenly, while adding 2-thiophenecarboxylic acid hydrazide and stirring, adding 0.05-0.2 molar equivalent of Et3N relative to 2-thiophenecarboxylic acid hydrazide to the active ester intermediate solution according to the amount of 2-thiophenecarboxylic acid hydrazide added, then, maintaining the reaction at 0°C and stirring at a uniform speed for 6 to 8 hours to ensure sufficient mixing and reaction, and obtaining a mixed solution containing the first corrosion inhibitor; S6. Extracting, drying, and separating the mixed solution containing the first corrosion inhibitor to obtain a high-purity first corrosion inhibitor.

8. Use of the corrosion inhibitor composition according to any one of claims 1 to 5 in oil and gas gathering and transportation.

Citation Information

Patent Citations

  • Green compound corrosion inhibitor containing Schiff base compound and application thereof

    CN112323070A

  • Acylhydrazone organic corrosion inhibitor, preparation method and application of acylhydrazone organic corrosion inhibitor in epoxy coating

    CN116239585A

  • Corrosion inhibitor for oil field and preparation method thereof

    CN117720898A

  • Aminosilane salts and silanamides of carboxylic acids as corrosion inhibitors

    CN1189849A

  • Corrosive poison composition

    CN1406988A