Preparation method of aramid fiber and aramid fiber

Through the steps of solution preparation, hydrogelation, freezing treatment, fiber growth, solvent replacement and drying, the problems of complicated preparation process and poor performance of aramid fiber are solved, and the aromatic fiber with larger specific surface area and smaller average pore diameter is achieved. Polyester fiber, suitable for thermal insulation and fire protection fields.

CN118835338APending Publication Date: 2024-10-25MICROMACRO ADVANCED MEMBRANE CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411139323.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

The existing aramid fiber preparation process is complex and cumbersome, making it difficult to achieve large-scale mass production. Moreover, conventional aramid fibers have small specific surface area, large average pore size, and poor performance.

Method used

Using the steps of solution preparation, hydrogelation, freezing treatment, fiber growth, solvent replacement and drying, and by selecting the appropriate solvent ratio and stirring speed, aramid fibers with larger specific surface area and smaller average pore diameter are formed.

Benefits of technology

It simplifies the preparation process of aramid fiber, increases its specific surface area and average pore size, has excellent performance, and is suitable for the fields of heat insulation and fire protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835338A_ABST
    Figure CN118835338A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of aramid fiber and the aramid fiber. The preparation method comprises the following steps: S1, solution preparation: preparing an aramid fiber solution; s2, hydrogel, to be more specific, dropwise adding a gelation reagent into the aramid solution to mix the two to obtain a hydrogel solution; wherein the gelation reagent comprises an organic solvent A and water; s3, freezing treatment: freezing the hydrogel liquid to obtain hydrogel; s4, fiber growth: adding the hydrogel into a coagulating bath reagent for aramid fiber growth to obtain aramid wet fibers; wherein the coagulating bath reagent comprises an organic solvent B and water; s5, solvent replacement: carrying out solvent replacement on the aramid wet fibers to obtain an aramid fiber precursor; and S6, drying: drying the aramid fiber precursor to obtain the aramid fiber. The aramid fiber prepared by the method is larger in specific surface area, smaller in average pore size and excellent in performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aramid fibers, and in particular to a preparation method of aramid fibers and the aramid fibers. Background Art

[0002] Aramid fiber can be used for fireproof and heat-insulating materials. Most of the current inventions for preparing aramid fiber use para-aramid as the raw material for synthesis, and the synthesis process mostly includes dry material dissolution, wet spinning, gelation, solvent replacement, drying and other steps. In the process of making aramid fiber, a wet spinning process is required, which has high requirements for technical equipment, a relatively complicated process, difficult operation, and difficult to use for large-scale mass production. Summary of the invention

[0003] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing aramid fiber and aramid fiber, and aramid fiber prepared by the method, which solves the problem of complex and cumbersome preparation process of conventional aramid fiber, and achieves the technical effect of larger specific surface area, smaller average pore size and excellent performance of aramid fiber.

[0004] The purpose of the present invention is achieved through the following technical solutions:

[0005] A method for preparing aramid fiber comprises the following steps:

[0006] S1. Solution preparation: preparing aramid solution;

[0007] S2, hydrogelation: adding a gelling agent to the aramid solution to mix the two to obtain a hydrogel solution; wherein the gelling agent includes an organic solvent A and water;

[0008] S3, freezing treatment: freezing the hydrogel liquid to obtain a hydrogel body;

[0009] S4, fiber growth: adding the hydrogel to a coagulation bath reagent to grow aramid fibers to obtain aramid wet fibers; wherein the coagulation bath reagent comprises an organic solvent B and water;

[0010] S5, solvent replacement: performing solvent replacement on the wet aramid fiber to obtain an aramid fiber precursor;

[0011] S6. Drying: Drying the aramid fiber precursor to obtain aramid fiber.

[0012] In one embodiment, in step S1, the aramid dry material is dissolved in a composite solvent to obtain the aramid solution; wherein the composite solvent includes an organic solvent C.

[0013] In one embodiment, the composite solvent further includes a strong base, and the mass ratio of the aramid dry material to the organic solvent C is (15-25):(300-400), and / or the mass ratio of the aramid dry material to the strong base is (15-25):(5-15).

[0014] In one embodiment, the composite solvent further includes water, and the mass ratio of the organic solvent C to water is (300-400):(40-80).

[0015] In one embodiment, in step S2, the mass ratio of the organic solvent A to water is (40-60): (40-60).

[0016] In one embodiment, in step S2, the mass ratio of the gelling agent to the aramid solution is (20-40): (60-130).

[0017] In one embodiment, in step S2, mixing is performed by stirring, and the stirring speed is 500-1000 r / min.

[0018] In one embodiment, in step S3, freezing the hydrogel liquid includes adding liquid nitrogen into the hydrogel liquid, and the hydrogel liquid is frozen by the liquid nitrogen to become the hydrogel body.

[0019] In one embodiment, the freezing of the hydrogel liquid also includes pre-freezing, wherein the hydrogel liquid is placed in a freezing chamber for a freezing at a temperature of -10°C to -50°C and a freezing time of 2h to 8h; and then the liquid nitrogen is added to the hydrogel liquid obtained by the freezing.

[0020] In one embodiment, in step S4, the mass ratio of the organic reagent B to water is (40-60): (40-60).

[0021] In one embodiment, in step S4, the mass ratio of the coagulation bath reagent to the hydrogel is (500-1000):(20-80).

[0022] In one embodiment, in step S4, the aramid fiber is grown for 3 hours to 10 hours.

[0023] In one embodiment, in step S5, the solvent used in the solvent replacement is a polar solvent.

[0024] In one embodiment, the organic solvent A, the organic solvent B and the organic solvent C are the same or different and are independently selected from any one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylhexanamide, N-methylpyrrolidone and triethyl phosphate.

[0025] The present invention also provides an aramid fiber, which is prepared by the above-mentioned method for preparing the aramid fiber.

[0026] In one embodiment, the specific surface area of ​​the aramid fiber is 100 m 2 / g~500m 2 / g, and the average pore size of the aramid fiber is 1 to 100 nm.

[0027] The beneficial effects of the present invention are as follows: aramid fibers are obtained through the preparation steps of solution preparation, hydrogelation, freezing treatment, fiber growth, solvent replacement and drying in sequence, thereby solving the problem of the complicated and cumbersome preparation process of conventional aramid fibers, and the prepared aramid fibers have a larger specific surface area, a smaller average pore size, and excellent performance, and are better applied in the fields of heat insulation and fire prevention. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 is a diagram of the aramid fiber during the growth process of Example 1 of the present invention;

[0030] Figure 2 This is a physical sample picture of the finished aramid fiber of Example 1;

[0031] Figure 3 This is a SEM image of the finished aramid fiber of Example 1 with a pixel size of 1.00 mm;

[0032] Figure 4 This is a SEM image of the finished aramid fiber of Example 1 with a pixel size of 500 μm. DETAILED DESCRIPTION

[0033] The specific embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the description of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The present invention provides a method for preparing aramid fiber, comprising the following steps:

[0035] S1. Solution preparation: preparing aramid solution;

[0036] S2, hydrogelation: adding a gelling agent to the aramid solution to mix the two to obtain a hydrogel solution; wherein the gelling agent includes an organic solvent A and water;

[0037] S3, freezing treatment: freezing the hydrogel liquid to obtain a hydrogel body;

[0038] S4, fiber growth: adding the hydrogel to a coagulation bath reagent to grow aramid fibers to obtain aramid wet fibers; wherein the coagulation bath reagent includes an organic solvent B and water;

[0039] S5, solvent replacement: performing solvent replacement on the wet aramid fiber to obtain an aramid fiber precursor;

[0040] S6. Drying: Drying the aramid fiber precursor to obtain a finished aramid fiber.

[0041] In this embodiment, aramid fiber is obtained through the preparation steps of solution preparation, hydrogelation, freezing treatment, fiber growth, solvent replacement and drying in sequence, which solves the problem of complex and tedious preparation process of conventional aramid fiber. The prepared aramid fiber has a larger specific surface area, a smaller average pore size, and excellent performance, and is better applied in the fields of heat insulation and fire prevention.

[0042] In step S1, an aramid solution is obtained by an organic polymerization reaction, or an aramid dry material is dissolved in a composite solvent to obtain an aramid solution, wherein the composite solvent includes an organic solvent C, and the organic solvent C is any one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylhexanamide, N-methylpyrrolidone and triethyl phosphate. Among them, the aramid solution is obtained by an organic polymerization reaction. In the aramid solution formed by direct polymerization, there is an excess of reactants, the aramid solution is viscous, and it is difficult to operate, and the aramid fiber prepared subsequently has poor effect. Therefore, it is preferred to dissolve the aramid dry material in a composite solvent to obtain an aramid solution, and the aramid dry material can be obtained by direct purchase. The dissolution of aramid dry material is a physical means and does not involve a chemical reaction process.

[0043] Furthermore, the composite solvent further includes a strong base, and the mass ratio of the aramid dry material to the organic solvent C is (15-25): (300-400), and / or the mass ratio of the aramid dry material to the strong base is (15-25): (5-15), that is, the mass ratio of the aramid dry material, the organic solvent C and the strong base is (15-25): (300-400): (5-15), or (18-22): (340-380): (8-12). The strong base is added to the composite solvent to accelerate the dissolution of the aramid dry material in the organic solvent C. The strong base can be selected from one or more of NaOH and KOH.

[0044] Furthermore, the composite solvent also includes water, and the mass ratio of the organic solvent C to water is (300-400): (40-80), or (340-380): (55-65). The solubility of the strong base in the organic solvent is low, and adding a small amount of water can increase the solubility of the strong base in the composite solvent. Among them, the mass ratio of the aramid dry material, the organic solvent C, the strong base and water is (15-25): (300-400): (5-15): (40-80), or (18-22): (340-380): (8-12): (55-65). Specifically, 20 g of aramid dry material, 360 g of N, N-dimethylacetamide (DMAC), 10 g of KOH, and 60 g of H2O can be used to obtain an aramid solution. 15 g, 18 g, 22 g, or 25 g of aramid dry material, 300 g, 340 g, 380 g, or 400 g of N, N-dimethylacetamide (DMAC), 5 g, 8 g, 12 g, or 15 g of KOH, and 40 g, 55 g, 65 g, or 80 g of H2O can also be used to obtain an aramid solution. The examples are not listed here.

[0045] Furthermore, in step S1, stirring is required when preparing the aramid solution, and the stirring time is 10 to 20 hours, or 10 to 14 hours; the stirring speed is 200 to 800 r / min, or 350 to 500 r / min. Sufficient stirring is required to completely dissolve the aramid dry material in the composite solvent to form an aramid solution.

[0046] In step S2, the mass ratio of organic solvent A to water is (40-60): (40-60). The organic solvent A is any one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylhexanamide, N-methylpyrrolidone and triethyl phosphate. Specifically, a gelling agent with a mass ratio of DMAC:H2O=50:50 can be prepared, or 40g or 60g of organic solvent A and 40g or 60g of water can be selected to obtain a gelling agent, which are not listed here one by one.

[0047] Further, in step S2, the mass ratio of the gelling agent to the aramid solution is (20-40): (60-130), or (25-35): (90-110). Specifically, 30 g of the gelling agent and 100 g of the aramid solution can be mixed to obtain a hydrogel solution, or 20 g, 25 g, 35 g or 40 g of the gelling agent and 60 g, 90 g, 110 g or 130 g of the aramid solution can be mixed to obtain a hydrogel solution, which are not listed here one by one.

[0048] Furthermore, in step S2, mixing is performed by stirring at a speed of 500 to 1000 r / min, or 600 to 800 r / min. In step S2, in order to make the aramid solution form a hydrogel solution in a critical translucent state, a high stirring speed needs to be maintained during the process of adding the gelling agent to the aramid solution. That is, stirring is necessary, otherwise the aramid solution will turn white and precipitate when encountering the gelling agent, and cannot be gelled.

[0049] In step S3, freezing the hydrogel liquid includes adding liquid nitrogen into the hydrogel liquid, and the hydrogel liquid becomes a hydrogel after being frozen by the liquid nitrogen. The mass ratio of the hydrogel liquid to the liquid nitrogen is (20-80):(40-100), or (40-80):(40-60).

[0050] Furthermore, freezing the hydrogel liquid also includes pre-freezing, in which the hydrogel liquid is placed in a freezing chamber for a freezing at a temperature of -10°C to -50°C, or -25°C to -40°C; the freezing time is 2h to 8h, or 3h to 5h; and liquid nitrogen is added to the hydrogel liquid after the freezing.

[0051] Specifically, in step S3, the hydrogel liquid is placed in a freezing chamber for pre-freezing, and then liquid nitrogen is added to the hydrogel liquid after the first freezing, and it is frozen again until the surface of the hydrogel liquid is frozen hard. The hydrogel liquid is pre-frozen so that when liquid nitrogen is added later, a better freezing effect can be achieved. Liquid nitrogen is added to make the hydrogel liquid freeze into a (semi) solid and then sink directly to the bottom after being put into a coagulation bath reagent. Among them, 50g of liquid nitrogen can be added to 50g of hydrogel liquid after the first freezing and frozen again; of course, 40g, 60g or 100g of liquid nitrogen can also be added to 20g, 40g or 80g of hydrogel liquid after the first freezing, which are not listed here one by one.

[0052] In step S4, the mass ratio of organic reagent B and water is (40-60): (40-60). Among them, organic solvent B is any one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylhexanamide, N-methylpyrrolidone and triethyl phosphate. The characteristics of aramid are hydrophilic but insoluble in water. The aramid in the hydrogel liquid will become solid when it encounters the water in the coagulation bath reagent, and solidify and grow fibers in the coagulation bath reagent. Specifically, a coagulation bath reagent with a mass ratio of DMAC:H2O=50:50 or DMAC:H2O=55:45 can be prepared, or 40g or 60g of organic solvent B and 40g or 60g of water can be selected to obtain a coagulation bath reagent, which will not be listed here one by one.

[0053] Further, in step S4, the mass ratio of the coagulation bath reagent and the hydrogel is (500-1000): (20-80), or (600-800): (40-80). It is necessary to make the hydrogel liquid (semi-solid) with a frozen surface, that is, the hydrogel is completely immersed in the coagulation bath reagent, so that the aramid fiber grows in the coagulation bath reagent to obtain aramid wet fiber, so the amount of coagulation bath reagent is relatively large. Specifically, 50g of hydrogel can be added to 600g of coagulation bath reagent for aramid fiber growth, or 20g, 40g or 80g of hydrogel can be added to 500g, 600g or 800g of coagulation bath reagent for aramid fiber growth, which are not listed here one by one.

[0054] Furthermore, in step S4, the growth time of the aramid fiber is 3 hours to 10 hours, or 5 hours to 8 hours, and sufficient time is required to ensure that the aramid fiber grows fully, and this process does not require stirring.

[0055] In step S5, the solvent used for solvent replacement is a polar solvent, which can be water. The number of solvent replacement treatments is 3 to 10 times, or 5 to 8 times; the time for solvent replacement treatment is 1 to 8 hours / time, or 4 to 6 hours / time. The purpose of solvent replacement is to remove the residual organic solvent introduced in the previous step in the grown aramid fiber, so as to facilitate the subsequent drying treatment in S6.

[0056] Furthermore, tert-butyl alcohol can be used as the solvent for solvent replacement, and the time for solvent replacement treatment using tert-butyl alcohol as the solvent is 6 to 15 hours, or 10 to 14 hours. When tert-butyl alcohol is used for solvent replacement, only one replacement is performed.

[0057] In step S6, the aramid fiber precursor is dried by freeze drying.

[0058] In the above embodiment, organic solvent A, organic solvent B and organic solvent C can be selected from the same or different organic solvents, and organic solvent A, organic solvent B and organic solvent C can be independently selected from any one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylhexanamide, N-methylpyrrolidone and triethyl phosphate. Among them, when the content of organic solvent A in the aramid solution is relatively large, only water can be added to the aramid solution as a gelling agent, and a hydrogel solution can also be obtained.

[0059] The present invention also provides an aramid fiber, which is prepared by the above-mentioned method for preparing the aramid fiber.

[0060] In one embodiment, the specific surface area of ​​the aramid fiber is 100 m 2 / g~500m 2 / g, the average pore size of aramid fiber is 1~100nm.

[0061] The following is further described by Examples 1-8 and Comparative Example 1.

[0062] Example 1

[0063] S1. Dissolution: Take 20g aramid dry material, 360g N,N-dimethylacetamide (DMAC), 10g KOH and 60g H2O and put them in a beaker. Stir at 400r / min for 12h until the aramid dry material is completely dissolved into aramid solution. The aramid dry material used is the meta-aramid raw material produced by our company.

[0064] S2. Hydrogelation: Prepare 30 g of a gelling agent with a mass ratio of DMAC:H2O=50:50, take 100 g of the above aramid solution, and then stir at a speed of 600 r / min, during which the gelling agent is continuously added dropwise until the aramid solution becomes translucent, to obtain a hydrogel solution.

[0065] S3. Freezing treatment: Pour the above 50 g of the hydrogel liquid into a glass dish, and then put it into a low-temperature freezer (-30° C.) for 3 hours. Then take it out and pour 50 g of liquid nitrogen on the surface of the hydrogel liquid until the surface of the hydrogel liquid is frozen.

[0066] S4. Fiber growth: 600 g of a coagulation bath reagent with a mass ratio of DMAC:H2O=55:45 was prepared, and the hydrogel liquid (semi-solid state) after the surface was frozen was added to the coagulation bath reagent to carry out the process of aramid fiber growth, and the process lasted for 5 hours.

[0067] S5, solvent replacement: the grown aramid fiber is put into deionized water for solvent replacement, the water is changed every 5 hours, and the replacement is performed 6 times. After the replacement with water is completed, the aramid fiber is put into tert-butyl alcohol for solvent replacement, and the tert-butyl alcohol replacement time lasts for 12 hours to obtain an aramid fiber precursor.

[0068] S6, drying: freeze-drying the replaced aramid fiber precursor to obtain a finished aramid fiber.

[0069] Example 2

[0070] The difference from Example 1 is that

[0071] S2. Hydrogelation: Prepare 40 g of a gelling agent with a mass ratio of DMAC:H2O=50:50, take 120 g of the above aramid solution, and then stir at a speed of 500 r / min, during which the gelling agent is continuously added dropwise until the aramid solution becomes translucent, to obtain a hydrogel solution.

[0072] S3. Freezing treatment: Pour the above 50 g of the hydrogel liquid into a glass dish, and then put it into a low-temperature freezer (-40° C.) for 5 hours. Then take it out and pour 60 g of liquid nitrogen onto the surface of the hydrogel liquid until the surface of the hydrogel liquid is frozen.

[0073] Example 3

[0074] The difference from Example 1 is that

[0075] S1. Dissolution: Take 15g aramid dry material, 300g N,N-dimethylacetamide (DMAC), 5g KOH and 40g H2O and put them in a beaker. Stir at 400r / min for 12h until the aramid dry material is completely dissolved into aramid solution. The aramid dry material used is the meta-aramid raw material produced by our company.

[0076] S2. Hydrogelation: Prepare 20 g of a gelling agent with a mass ratio of DMAC:H2O=40:60, take 60 g of the above aramid solution, and then stir at a speed of 600 r / min, during which the gelling agent is continuously added dropwise until the aramid solution becomes translucent, to obtain a hydrogel solution.

[0077] Example 4

[0078] The difference from Example 1 is that

[0079] S1. Dissolution: Take 25g aramid dry material, 300g N,N-dimethylacetamide (DMAC), 5g KOH, and 40g H2O and put them in a beaker. Stir at 400r / min for 12h until the aramid dry material is completely dissolved into aramid solution. The aramid dry material used is the meta-aramid raw material produced by our company.

[0080] S2. Hydrogelation: Prepare 40 g of a gelling agent with a mass ratio of DMAC:H2O=60:40, take 130 g of the above aramid solution, and then stir at a speed of 1000 r / min, during which the gelling agent is continuously added dropwise until the aramid solution becomes translucent, to obtain a hydrogel solution.

[0081] Example 5

[0082] The difference from Example 1 is that

[0083] S1. Dissolution: Take 25g aramid dry material, 400g N,N-dimethylacetamide (DMAC), 15g KOH and 80g H2O and put them in a beaker. Stir at 400r / min for 12h until the aramid dry material is completely dissolved into aramid solution. The aramid dry material used is the meta-aramid raw material produced by our company.

[0084] S2. Hydrogelation: Prepare 40 g of a gelling agent with a mass ratio of DMAC:H2O=50:50, take 130 g of the above aramid solution, and then stir at a speed of 600 r / min, during which the gelling agent is continuously added dropwise until the aramid solution becomes translucent, to obtain a hydrogel solution.

[0085] Example 6

[0086] The difference from Example 1 is that

[0087] S3. Freezing treatment: Pour the above 20 g of the hydrogel liquid into a glass dish, and then put it into a low-temperature freezer (-10°C) for 8 hours, then take it out and pour 40 g of liquid nitrogen on the surface of the hydrogel liquid until the surface of the hydrogel liquid is frozen.

[0088] S4. Fiber growth: 500 g of a coagulation bath reagent with a mass ratio of DMAC:H2O=40:60 was prepared, and the hydrogel liquid (semi-solid state) after the surface was frozen was added to the coagulation bath reagent to carry out the process of aramid fiber growth, and the process lasted for 3 hours.

[0089] Example 7

[0090] The difference from Example 1 is that

[0091] S3. Freezing treatment: Pour the above 80 g of the hydrogel liquid into a glass dish, and then put it into a low-temperature freezer (-50° C.) for 2 hours, then take it out and pour 100 g of liquid nitrogen onto the surface of the hydrogel liquid until the surface of the hydrogel liquid is frozen.

[0092] S4. Fiber growth: 1000 g of a coagulation bath reagent with a mass ratio of DMAC:H2O=60:40 was prepared, and the hydrogel liquid (semi-solid state) after the surface was frozen was added to the coagulation bath reagent to carry out the process of aramid fiber growth, and the process lasted for 10 hours.

[0093] Example 8

[0094] The difference from Example 1 is that

[0095] S3. Freezing treatment: No need for pre-freezing treatment, pour 50 g of the above hydrogel solution into a glass dish, pour 50 g of liquid nitrogen onto the surface of the hydrogel solution until the surface of the hydrogel solution is frozen.

[0096] Comparative Example 1

[0097] The difference from Example 1 is that

[0098] S2. Hydrogelation: Prepare 50 g of a gelling agent with a mass ratio of DMAC:H2O=50:50, take 100 g of the above aramid solution, and then stir at a speed of 600 r / min, during which the gelling agent is continuously added dropwise until the aramid solution becomes translucent, to obtain a hydrogel solution.

[0099] S3. Freezing treatment: Pour 50 g of the above hydrogel solution into a glass dish, and then place it in a low-temperature freezer (-30° C.) for 3 hours.

[0100] The experimental data of Examples 1-8 and Comparative Example 1 are shown in Table 1.

[0101] Table 1 Experimental data table

[0102]

[0103]

[0104] Performance Test:

[0105] (1) The equipment used to collect the SEM images of Example 1 is: field emission scanning electron microscope SU8010, supplier: MP (MACAO COMMERCIAL OFFSHORE). Through analysis, it can be known that: Figure 1 This is a diagram of the growth process of the aramid fiber of Example 1 in the coagulation bath reagent, and the aramid fiber grows well; Figure 2 This is a physical sample picture of the finished aramid fiber of Example 1; Figure 3 This is a SEM image of the finished aramid fiber of Example 1 with a pixel size of 1.00 mm. It can be seen that the finished aramid fiber is in a fibrous shape; Figure 4 This is a SEM image of the finished aramid fiber of Example 1 with a pixel size of 500 μm. It can be seen that the surface of the finished aramid fiber has a microporous structure.

[0106] The specific surface area and average pore size of the aramid fibers prepared in Example 1 and Comparative Example 1 were tested by the BET test method (the instrument was a specific surface area and pore size analyzer, supplier: Hangzhou New Blue Technology Co., Ltd., specification model: JW-BK-400), and the data shown in Table 2 were obtained.

[0107] Table 2 Specific surface area and pore size data of Example 1 and Comparative Example 1

[0108] Test content Example 1 Comparative Example 1 <![CDATA[BET multi-point specific surface area ((m 2 / g))]]> 144.199 28.20 Average adsorption pore size (nm) 19.51 11.109 BJH adsorption average pore size (nm) 16.954 8.215 BJH desorption average pore size (nm) 30.213 8.64

[0109] It can be seen from Table 2 that the specific surface area of ​​the finished aramid fiber of Example 1 is 144.199 m 2 / g, the average adsorption pore size is 19.51nm, and the finished aramid fiber has excellent performance; the specific surface area of ​​the aramid fiber prepared in Comparative Example 1 is only 28.2m 2 / g, which is much lower than the result in Example 1.

[0110] Among them, the principle of fiber formation:

[0111] The hydrogel solution obtained in step 2 is a semi-transparent critical state aramid solution. The so-called critical state means that if a gelling agent is added at this time, the aramid solution will immediately form a white powder precipitate. This state is also the state with the lowest aramid concentration. The hydrogel solution in this state is frozen with liquid nitrogen and added to the coagulation bath. The frozen semi-solid aramid solution will sink to the bottom. At this time, the aramid molecules are difficult to stack tightly due to their low concentration. After encountering the coagulation bath solution, they will solidify to form a fibrous solid. Since the density of aramid fiber is less than the density of the coagulation bath liquid, it will gradually grow upward under the action of buoyancy to form aramid fiber (reference Figure 1 ).

[0112] In summary, the present invention can prepare aramid fibers with excellent performance through a simple process flow, and the equipment used has low energy consumption.

[0113] The above are only preferred embodiments of the present invention, and are not intended to limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with this profession can make some changes or modifications to the technical contents disclosed above without departing from the scope of the technical solution of the present invention, which are equivalent embodiments of equivalent changes. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing aramid fiber, characterized in that: The following steps are involved: S1. Solution preparation: preparing aramid solution; S2, hydrogelation: adding a gelling agent to the aramid solution to mix the two to obtain a hydrogel solution; wherein the gelling agent includes an organic solvent A and water; S3, freezing treatment: freezing the hydrogel liquid to obtain a hydrogel body; S4, fiber growth: adding the hydrogel to a coagulation bath reagent to grow aramid fibers to obtain aramid wet fibers; wherein the coagulation bath reagent comprises an organic solvent B and water; S5, solvent replacement: performing solvent replacement on the wet aramid fiber to obtain an aramid fiber precursor; S6. Drying: Drying the aramid fiber precursor to obtain aramid fiber.

2. The method for preparing aramid fiber according to claim 1, characterized in that: In step S1, the aramid dry material is dissolved in a composite solvent to obtain the aramid solution; wherein the composite solvent includes an organic solvent C.

3. The method for preparing aramid fiber according to claim 2, characterized in that: The composite solvent also includes a strong base, and the mass ratio of the aramid dry material to the organic solvent C is (15-25): (300-400), and / or the mass ratio of the aramid dry material to the strong base is (15-25): (5-15).

4. The method for preparing aramid fiber according to claim 3, characterized in that: The composite solvent also includes water, and the mass ratio of the organic solvent C to water is (300-400): (40-80).

5. The method for preparing aramid fiber according to claim 1, characterized in that: In step S2, the mass ratio of the organic solvent A to water is (40-60): (40-60).

6. The method for preparing aramid fiber according to claim 1, characterized in that: In step S2, the mass ratio of the gelling agent to the aramid solution is (20-40): (60-130).

7. The method for preparing aramid fiber according to claim 1, characterized in that: In step S2, mixing is performed by stirring, and the stirring speed is 500-1000 r / min.

8. The method for preparing aramid fiber according to claim 1, characterized in that: In step S3, the freezing of the hydrogel liquid includes adding liquid nitrogen into the hydrogel liquid, and the hydrogel liquid is frozen by the liquid nitrogen to become the hydrogel body.

9. The method for preparing aramid fiber according to claim 8, characterized in that: The freezing of the hydrogel liquid also includes pre-freezing, in which the hydrogel liquid is placed in a freezing chamber for a freezing at a temperature of -10°C to -50°C for a freezing time of 2h to 8h; and then the liquid nitrogen is added to the hydrogel liquid obtained by the freezing.

10. The method for preparing aramid fiber according to claim 1, characterized in that: In step S4, the mass ratio of the organic reagent B to water is (40-60): (40-60).

11. The method for preparing aramid fiber according to claim 1, characterized in that: In step S4, the mass ratio of the coagulation bath reagent to the hydrogel is (500-1000):(20-80).

12. The method for preparing aramid fiber according to claim 1, characterized in that: In step S4, the aramid fiber is grown for 3 hours to 10 hours.

13. The method for preparing aramid fiber according to claim 1, characterized in that: In step S5, the solvent used for the solvent replacement is a polar solvent.

14. The method for preparing aramid fiber according to claim 2, characterized in that: The organic solvent A, the organic solvent B and the organic solvent C are the same or different and are independently selected from one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylhexanamide, N-methylpyrrolidone and triethyl phosphate.

15. An aramid fiber, characterized in that: The aramid fiber is prepared by the preparation method of any one of claims 1 to 14.

16. The aramid fiber according to claim 15, characterized in that: The specific surface area of ​​the aramid fiber is 100 m 2 / g~500m 2 / g, and the average pore size of the aramid fiber is 1 to 100 nm.