Secondary cutting processing and cleaning method for monocrystalline silicon wafer

By using polyethylene glycol as an adhesive and laser cutting technology, combined with ultrasonic cleaning and temperature control, the problem of mechanical damage and debris risk in secondary cutting of single crystal silicon wafers is solved, and efficient, low-cost non-destructive dimensional processing is achieved .

CN118841318APending Publication Date: 2024-10-25ZHEJIANG HAINA SEMICON CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410785979.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

During the secondary cutting process of single crystal silicon wafers, traditional laser cutting will cause mechanical damage to the polished surface and spark sputtering, and the surface tension of the bonded silicon wafers is large, making it difficult to separate, increasing the risk of fragmentation. Traditional methods are costly and The operation is complicated.

Method used

Polyethylene glycol is used as the adhesive and is evenly coated on the surface of the silicon wafer through the spin coating process. After bonding the two silicon wafers, they are positioned through a positioning frame, cut using a laser cutting machine, and the silicon wafers are cleaned through ultrasonic cleaning and temperature control. Separation, final chamfering and RCA standard cleaning.

Benefits of technology

It effectively reduces the mechanical damage to the polished surface during the cutting process, reduces the fragmentation rate, is easy to operate, has low cost, is suitable for non-destructive dimensional processing, and significantly improves processing efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841318A_ABST
    Figure CN118841318A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor monocrystalline silicon wafer substrate manufacturing, in particular to a secondary cutting processing and cleaning method of a monocrystalline silicon wafer. Comprising the following steps: carrying out RCA standard cleaning on a to-be-processed silicon wafer; uniformly coating polyethylene glycol on the surface of the silicon wafer through a spin-coating process; bonding the polished surfaces of the two monocrystalline silicon wafers together; the silicon wafer is positioned through the right-angle mold positioning frame; a laser cutting machine is adopted for cutting; carrying out ultrasonic cleaning on the silicon wafer by adopting SC-1 and H2O, and separating the bonded silicon wafer at the same time; carrying out edge chamfering processing on the processed silicon wafer; and cleaning the silicon wafer through an RCA standard cleaning process. According to the design, mechanical stripping is not needed in the separation process of the silicon wafer, the fragment rate is greatly reduced, the bonding and fragment separation process is controlled through temperature, operation is easy and convenient, the effect is remarkable, flexibility is high, and the method can be suitable for surface non-deformation size machining of the polished silicon wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor single crystal silicon wafer substrate manufacturing, in particular to a secondary cutting processing and cleaning method for a single crystal silicon wafer. Background Art

[0002] The monocrystalline silicon wafer substrate is the core material for manufacturing wafers. The monocrystalline silicon polished wafer is processed through multiple processes such as crystal growth, segmentation, rounding, slicing, chamfering, grinding, etching, back processing, polishing, cleaning, and inspection. The processing flow is complex and complicated. During the final inspection of the monocrystalline silicon polished wafer, it is usually defective due to factors such as crystal defects and physical damage to the edge. At this time, the silicon wafer needs to be resized to reduce economic losses. For example, an 8-inch polished silicon wafer with poor edges can be cut into a 6-inch or smaller silicon wafer. However, the traditional laser cutting process will inevitably cause mechanical damage to the polished surface. Sometimes the sputtering of sparks will also burn the surface of the polished wafer, causing deeper damage that is difficult to remove by cleaning.

[0003] In order to protect the polished surface of the silicon wafer during the secondary cutting process, the surface of the silicon wafer needs to be treated. However, the cost of methods such as sticking polymer films or coating is relatively high. Positioning and bonding the polished surfaces of two silicon wafers of the same specification can not only protect them from each other, but also allow the two silicon wafers to be cut at the same time. The polished surface has a lower roughness and stronger hydrophilicity, which makes the surface tension of the bonded silicon wafers larger and difficult to separate. Physical peeling is usually required, resulting in a greater risk of fragmentation. For example, during the silicon wafer polishing process, the silicon wafer needs to be bonded to the polishing disk with wax, and then mechanically scraped after polishing. The edges of silicon wafers of the same size completely overlap, making mechanical peeling difficult and posing a greater risk of fragmentation. In view of this, we propose a secondary cutting processing and cleaning method for single crystal silicon wafers. Summary of the invention

[0004] The object of the present invention is to provide a secondary cutting processing and cleaning method for a single crystal silicon wafer to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention aims to provide a secondary cutting and cleaning method for a single crystal silicon wafer, comprising the following steps:

[0006] S1. Pretreatment of monocrystalline silicon wafers: clean the silicon wafers to be processed according to RCA standards;

[0007] S2, wax coating: polyethylene glycol is evenly coated on the surface of the silicon wafer by spin coating process;

[0008] S3, wafer bonding: bonding the polished surfaces of two single crystal silicon wafers together;

[0009] S4, positioning: positioning the silicon wafer by a right-angle mold positioning frame;

[0010] S5, cutting: cutting is performed using a laser cutting machine;

[0011] S6, Sharding: Using SC-1 and H 2 O ultrasonically clean the silicon wafer and separate the bonded silicon wafers;

[0012] S7, chamfering: performing edge chamfering on the processed silicon wafer;

[0013] S8. Cleaning: Clean the silicon wafer using the RCA standard cleaning process.

[0014] As a further improvement of the technical solution, in step S1, the silicon wafer is a 4-12 inch polished silicon wafer. The beneficial effect is that the diameter sizes of the single crystal silicon polished wafers used to manufacture wafers are commonly 4 inches (100mm), 5 inches (125mm), 6 inches (150mm), 8 inches (200mm), and 12 inches (300mm). By resizing the silicon wafers with poor appearance such as edge collapse, notches, abrasions, scratches, or poor crystal parameters such as RRG and ORG, the poor polished wafers can be processed into usable small-sized polished silicon wafers, which have high economic value.

[0015] As a further improvement of the technical solution, in step S2, the molecular weight of the polyethylene glycol is 4000, the spin coating temperature is 65°C, the spin coating speed is 60r / min, and the spin coating time is 90s. The polyethylene glycol of 4000 is solid when it is below the crystallization temperature (48-52°C), showing a certain adhesive force, and is liquid when it is above the crystallization temperature. Moreover, the oligomer is easily soluble in water and common organic solvents, and the bonded silicon wafers can be separated by ultrasonic immersion in water or solvents above the crystallization temperature. The slicing process will not cause physical and mechanical damage to the surface of the silicon wafer, and it is easy to clean and remove the residual adhesive on the surface of the silicon wafer. Spin coating at 65°C can ensure that the polyethylene glycol is in a liquid state when spin coating, which is convenient for uniform coating, and the thickness of the liquid film can be effectively controlled by controlling the spin coating time and spin coating speed.

[0016] As a further improvement of the technical solution, in step S3, the bonding is to fit the polished surfaces of two silicon wafers of the same size and specification together. When fitting, the positioning edges or positioning grooves of the silicon wafers need to be aligned by positioning. By applying 2kg / cm 2The temperature is lowered to 25°C while the pressure is applied, and the two silicon wafers are bonded together through the crystallization of polyethylene glycol. The beneficial effect is that the size of the two silicon wafers when cut at the same time can be reduced by positioning and bonding the silicon wafers, and the two silicon wafers are pressed together by applying a certain pressure on the surface of the silicon wafers, and then the polyethylene glycol undergoes a liquid-solid transition by lowering the temperature, making it adhesive.

[0017] As a further improvement of the technical solution, in step S4, the positioning frame is a right-angle mold positioning frame, which can be used for positioning flat-edge and grooved silicon wafers. Its beneficial effect is that silicon wafers used to manufacture wafers usually have positioning edges or positioning grooves with a specific angle to the crystal direction. The positioning frame can accurately position the silicon wafers, reducing the deviation of the new positioning edges or positioning grooves after cutting.

[0018] As a further improvement of the technical solution, in step S5, the cutting method is laser cutting, and the laser cutting head is controlled by a pre-designed path to cut silicon wafers of different shapes and sizes; the power of the laser cutting is 100%, the cutting speed is 10-30 mm / s, and compressed air is used for blowing throughout the cutting process, and the air pressure of the compressed air is 3 MPa. The beneficial effect is that laser cutting can be used to cut pre-set paths and obtain cut silicon wafers of different specifications, and the processing speed can be easily controlled by adjusting the laser power and speed.

[0019] As a further improvement of the technical solution, in step S6, the cleaning is two-tank cleaning, the cleaning agent of the first tank is SC-1 cleaning solution, the cleaning temperature is 65°C, the cleaning time is 10 minutes, the ultrasonic frequency during cleaning is 40Hz, the stroke of the tossing cleaning is about 5cm, and the frequency is 20 times / min; the cleaning liquid of the second tank is pure water overflow cleaning, the cleaning time is 10 minutes, and the cleaning temperature is 25°C. Its beneficial effect is that the cleaning tank temperature is set to 65°C to ensure that the polyethylene glycol is converted into a liquid state, the polished surfaces of the two silicon wafers are separated by ultrasound and tossing, the SC-1 solution is dissolved and peeled off the silicon wafer surface, and the residual chemical reagents on the surface are removed by the cleaning tank of pure water overflow cleaning.

[0020] As a further improvement of the technical solution, in step S7, the chamfering process is rough chamfering + fine chamfering, and the chamfering removal amount is 0.5-1 mm. Its beneficial effect is that the mechanical damage caused by laser cutting on the edge of the silicon wafer can be removed by edge chamfering to obtain an ideal edge profile.

[0021] As a further improvement of the technical solution, in step S8, the cleaning is an RCA standard cleaning process, which has the beneficial effect of removing organic matter, particles, metal and other contaminants on the surface of the silicon wafer caused by the above series of processing through RCA standard cleaning.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] In the secondary cutting and cleaning method of the single crystal silicon wafer, two polished silicon wafers are bonded together by using a temperature-sensitive adhesive to protect each other, and then the two silicon wafers are laser cut at the same time, and then the silicon wafers are separated by increasing the temperature and ultrasound, and finally the polished silicon wafers with resized processing are obtained after chamfering and cleaning; in the separation process of the silicon wafers, no mechanical peeling is required, which greatly reduces the fragmentation rate, and the bonding and slicing process is controlled by temperature, which is simple to operate, has a significant effect, is highly flexible, and can be applicable to the surface non-destructive sizing processing of the polished silicon wafers. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is an exemplary overall method flow chart of the present invention;

[0025] Figure 2 is a schematic structural diagram of an exemplary silicon wafer to be processed in the present invention;

[0026] Figure 3 is an exemplary spin coating process operation flow chart of the present invention;

[0027] Figure 4 It is a schematic diagram of the structure of an exemplary double-layer single crystal silicon wafer after bonding in the present invention;

[0028] Figure 5 This is a schematic diagram of an exemplary silicon wafer positioning before cutting in the present invention;

[0029] Figure 6 This is a schematic diagram of the dimensions of an exemplary silicon wafer after cutting and chamfering in the present invention.

[0030] In the figure:

[0031] 1. Silicon wafer to be processed; 2. Suction cup; 3. Negative pressure pore; 4. Polyethylene glycol; 5. Polyethylene glycol quantitative dropper; 6. Polyethylene glycol liquid film; 7. Polyethylene glycol solid film; 8. Single crystal silicon wafer; 9. Bonded silicon wafer; 10. Positioning frame; 11. Bonded silicon wafer after cutting; 12. First cut silicon wafer; 13. Second cut silicon wafer. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] like Figure 1 As shown, this embodiment provides a secondary cutting processing and cleaning method for a single crystal silicon wafer, comprising the following steps:

[0035] S1. Pretreatment of monocrystalline silicon wafers: clean the silicon wafers to be processed according to RCA standards;

[0036] In this step, the silicon wafer is a 4-12 inch polished silicon wafer.

[0037] Specifically, common diameter sizes of single crystal silicon polishing wafers used to manufacture wafers are 4 inches (100mm), 5 inches (125mm), 6 inches (150mm), 8 inches (200mm), and 12 inches (300mm). By resizing silicon wafers with poor appearance such as edge collapse, notches, abrasions, scratches, or poor crystal parameters such as RRG and ORG, the poor polishing wafers can be processed into usable small-sized polished silicon wafers, which have high economic value.

[0038] S2, wax coating: polyethylene glycol is evenly coated on the surface of the silicon wafer by spin coating process;

[0039] In this step, the molecular weight of polyethylene glycol is preferably 4000, the spin coating temperature is 65° C., the spin coating speed is 60 r / min, and the spin coating time is 90 s.

[0040] Among them, 4000 polyethylene glycol is solid when it is below the crystallization temperature (48-52°C), showing a certain adhesive force, and it is liquid when it is above the crystallization temperature. Moreover, the oligomer is easily soluble in water and common organic solvents. The bonded silicon wafers can be separated by ultrasonic immersion in water or solvents above the crystallization temperature. The separation process will not cause physical and mechanical damage to the surface of the silicon wafer, and it is easy to clean and remove the residual adhesive on the surface of the silicon wafer. Spin coating at 65°C can ensure that the polyethylene glycol is in a liquid state during spin coating, which is convenient for uniform coating. The thickness of the liquid film can be effectively controlled by controlling the spin coating time and spin coating speed.

[0041] S3, wafer bonding: bonding the polished surfaces of two single crystal silicon wafers together;

[0042] In this step, the wafers are bonded together by placing the polished surfaces of two silicon wafers of the same size on each other. During bonding, the positioning edges or positioning grooves of the silicon wafers need to be aligned. A 2kg / cm 2 The pressure is then reduced to 25°C and the two silicon wafers are bonded together through the crystallization of polyethylene glycol.

[0043] Specifically, the size of two silicon wafers when cut at the same time can be reduced by positioning and bonding the silicon wafers. A certain pressure is applied to the surface of the silicon wafers to make the two silicon wafers stick together, and then the temperature is lowered to cause the polyethylene glycol to undergo a liquid-solid transition, making it adhesive.

[0044] S4, positioning: positioning the silicon wafer by a right-angle mold positioning frame;

[0045] In this step, the positioning frame is a right-angle mold positioning frame, which can be used for positioning flat-edge and grooved silicon wafers.

[0046] Specifically, silicon wafers used to manufacture wafers usually have positioning edges or positioning grooves with specific angles to the crystal direction. The silicon wafers can be accurately positioned by a positioning frame to reduce the deviation of new positioning edges or positioning grooves after cutting.

[0047] S5, cutting: cutting is performed using a laser cutting machine;

[0048] In this step, the cutting method is laser cutting, and the laser cutting head is controlled by a pre-designed path to cut silicon wafers of different shapes and sizes; the power of laser cutting is 100%, the cutting speed is 10-30 mm / s, and compressed air is used throughout the cutting process, and the compressed air pressure is 3 MPa.

[0049] Specifically, laser cutting can be used to perform cutting along a pre-set path and obtain cut silicon wafers of different specifications. The processing speed can be easily controlled by adjusting the laser power and speed.

[0050] S6, Sharding: Using SC-1 and H 2 O ultrasonically clean the silicon wafers and separate the bonded silicon wafers;

[0051] In this step, the cleaning is carried out in two tanks. The cleaning agent in the first tank is SC-1 cleaning liquid, the cleaning temperature is 65°C, the cleaning time is 10 minutes, the ultrasonic frequency during cleaning is 40Hz, the stroke of the scattering cleaning is about 5cm, and the frequency is 20 times / min; the cleaning liquid in the second tank is pure water overflow cleaning, the cleaning time is 10 minutes, and the cleaning temperature is 25°C.

[0052] Specifically, the temperature of the cleaning tank is set at 65°C to ensure that the polyethylene glycol is converted into liquid. The polished surfaces of the two silicon wafers are separated by ultrasound and polishing, and the SC-1 solution is used to dissolve it and peel it off the surface of the silicon wafer. The residual chemical reagents on the surface are then removed by a cleaning tank with pure water overflow.

[0053] S7, chamfering: performing edge chamfering on the processed silicon wafer;

[0054] In this step, the chamfering process is rough chamfering + fine chamfering, and the chamfering removal amount is 0.5 to 1 mm.

[0055] Specifically, the edge chamfering process can remove the mechanical damage on the edge of the silicon wafer caused by the laser cutting process, and obtain an ideal edge profile.

[0056] S8, cleaning: cleaning the silicon wafer using the RCA standard cleaning process;

[0057] In this step, the cleaning is performed using the RCA standard cleaning process.

[0058] Specifically, RCA standard cleaning is used to remove organic matter, particles, metal and other contaminants on the surface of the silicon wafer caused by the above series of processing.

[0059] In summary, the wax used for bonding the wafers is preferably polyethylene glycol (PEG6000), the cutting process is laser cutting, and the slicing process is to separate the combined silicon wafers after cutting by heating (greater than the melting point of polyethylene glycol) to cause the polyethylene glycol to undergo a solid-liquid transition. Compared with the traditional single-wafer cutting method, this solution effectively reduces the mechanical damage to the polished surface during the cutting process by bonding the two wafers. Using polyethylene glycol as an adhesive, the silicon wafers can be bonded and separated by controlling the temperature, without the need for shoveling or other mechanical separation, which greatly reduces the fragmentation rate of the silicon wafers. Polyethylene glycol is easily soluble in water and common organic solvents, which is convenient for cleaning and removal after processing. The method is reasonably designed and easy to operate, and can be used for surface non-destructive cutting of polished silicon wafers.

[0060] like Figure 2-Figure 6 As shown, this embodiment also provides a secondary cutting and cleaning method for a single crystal silicon wafer based on specific parameters, and the specific operation steps are as follows:

[0061] S1, select 20 silicon wafers 1 to be processed with a diameter of 200 mm and a thickness of 725 μm, place them in a PFA basket and perform RCA standard cleaning to obtain a clean silicon wafer surface;

[0062] S2, placing a clean silicon wafer 1 to be processed on a suction cup 2 of a spin coater, with a negative pressure pore 3 provided on the suction cup 2 for adsorbing the back of the silicon wafer 1 to be processed, and the polished surface of the silicon wafer 1 to be processed facing upward; a temperature control device is provided below the suction cup 2, and the temperature is controlled to be 65°C; polyethylene glycol 4 with a molecular weight of 4000 is heated to a liquid state in a water bath at 60°C, and is quantitatively added to the silicon wafer 1 to be processed through a polyethylene glycol quantitative dropper 5, and the amount of the drop is 2.0g; the polyethylene glycol liquid film 6 is obtained by spin coating at 60r / min for 1min using a spin coater;

[0063] S3, laminating the polished surface of another single crystal silicon wafer 8 of the same size and specification as the silicon wafer 1 to be processed with the silicon wafer 1 processed in step S2 after positioning the flat edge of the silicon wafer, placing it in a room temperature environment for natural cooling after laminating, and during the cooling process, the polyethylene glycol liquid film 6 undergoes a liquid-solid transformation into a polyethylene glycol solid film 7, thereby bonding the silicon wafer 1 to be processed and the single crystal silicon wafer 8 of the same size and specification to form a laminated silicon wafer 9 consisting of a double layer of single crystal silicon wafers;

[0064] S4, placing the bonded silicon wafer 9 on the positioning frame 10 for positioning. The positioning frame 10 is in the shape of a right angle ruler. To facilitate positioning, the thickness of each frame of the positioning frame 10 is preferably 5 mm;

[0065] S5. A commercial laser cutting machine is selected, and the cutting process is set as follows: cutting rate 15 mm / s, peak power 100%, duty cycle 95%, cutting gas is air, air pressure 3 MPa, cutting height 2 mm / s, and upper stage height 10 mm / s; the cutting path is set by the laser cutting machine, and the final cutting diameter is set to 150.7 mm; the positioned bonded silicon wafer 9 is cut by the above process to obtain the cut bonded silicon wafer 11;

[0066] S6. Put the cut bonded silicon wafer 11 into a cleaning basket for cleaning. The first tank uses SC-1 solution, the cleaning temperature is 65°C, the ultrasonic power is 1.5kW, the ultrasonic frequency is 40Hz, and the cleaning time is 10min. Through this step of cleaning, the polyethylene glycol 4 in the cut bonded silicon wafer 11 is completely peeled off the surface of the silicon wafer, and the cut bonded silicon wafer 11 is separated into two silicon wafers again. At this time, the polished surfaces of the two silicon wafers are placed opposite to each other in a card slot in the basket; the above two silicon wafers are placed in the same direction in the cleaning basket, with one silicon wafer placed in each card slot, and then transferred to the pure water overflow tank for cleaning. The cleaning temperature is 25°C and the cleaning time is 10min.

[0067] S7, select a commercial chamfering machine, and use a conventional chamfering process to perform edge chamfering on the two silicon wafers obtained in step S6, with a chamfering removal amount of 0.7 um, and after chamfering, obtain two first cut silicon wafers 12 and second cut silicon wafers 13 with undamaged edges;

[0068] S8. The first cut silicon wafer 12 and the second cut silicon wafer 13 are cleaned by using the RCA standard cleaning process, and after the cleaning, finished second cut silicon wafers are obtained.

[0069] Specifically, the adhesive used in the method is common low-cost polyethylene glycol. The characteristics of this oligomer are that it is solid when it is below the crystallization temperature (48-52°C), showing a certain adhesive force, and it is liquid when it is above the crystallization temperature. In addition, the oligomer is easily soluble in water and common organic solvents. The bonded silicon wafers can be separated by ultrasonically immersing them in water or solvents above the crystallization temperature. The separation process will not cause physical and mechanical damage to the surface of the silicon wafer, and it is easy to clean and remove the residual adhesive on the surface of the silicon wafer.

[0070] Those skilled in the art will appreciate that the process of implementing all or part of the steps of the above embodiments may be completed by hardware, or may be completed by instructing related hardware through a program.

[0071] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A secondary cutting and cleaning method for a single crystal silicon wafer, It is characterized in that The steps include: S1. Pretreatment of monocrystalline silicon wafers: clean the silicon wafers to be processed according to RCA standards; S2, wax coating: polyethylene glycol is evenly coated on the surface of the silicon wafer by spin coating process; S3, wafer bonding: bonding the polished surfaces of two single crystal silicon wafers together; S4, positioning: positioning the silicon wafer by a right-angle mold positioning frame; S5, cutting: cutting is performed using a laser cutting machine; S6, Sharding: Using SC-1 and H 2 O ultrasonically clean the silicon wafers and separate the bonded silicon wafers; S7, chamfering: performing edge chamfering on the processed silicon wafer; S8. Cleaning: Clean the silicon wafer using the RCA standard cleaning process.

2. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 1, Features: In the step S1, the silicon wafer is a 4-12 inch polished silicon wafer.

3. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 1, Features: In the step S2, the molecular weight of the polyethylene glycol is 4000, the spin coating temperature is 65°C, the spin coating speed is 60 r / min, and the spin coating time is 90 s.

4. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 1, Features: In step S3, the bonding is to fit the polished surfaces of two silicon wafers of the same size and specification together. During the bonding, the positioning edges or positioning grooves of the silicon wafers need to be aligned by positioning. A 2kg / cm 2 The pressure is then reduced to 25°C while the temperature is lowered to allow the two silicon wafers to be bonded together through the crystallization of polyethylene glycol.

5. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 1, Features: In the step S4, the positioning frame is a right-angle mold positioning frame suitable for positioning flat-edge and grooved silicon wafers.

6. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 1, Features: In the step S5, the cutting method is laser cutting, and the laser cutting head is controlled by a pre-designed path to cut the silicon wafer into different shapes and sizes.

7. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 6, Features: The power of the laser cutting is 100%, the cutting speed is 10-30 mm / s, and compressed air is used for blowing throughout the cutting process, and the air pressure of the compressed air is 3 MPa.

8. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 1, Features: In step S6, the cleaning is performed in two tanks, the cleaning agent in the first tank is SC-1 cleaning solution, the cleaning temperature is 65°C, the cleaning time is 10 min, the ultrasonic cleaning frequency is 40 Hz, the scattering cleaning stroke is about 5 cm, and the frequency is 20 times / min; the cleaning solution in the second tank is pure water overflow cleaning, the cleaning time is 10 min, and the cleaning temperature is 65°C.

9. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 1, Features: In the step S7, the chamfering process is rough chamfering + fine chamfering, and the chamfering removal amount is 0.5-1 um.

10. The method for secondary cutting and cleaning of a single crystal silicon wafer according to claim 1, Features: In the step S8, the cleaning is an RCA standard cleaning process.

Citation Information

Cited By

  • IC process method capable of converting 8 inches into 6 inches and realizing accurate overlay

    CN116931381A

  • An IC manufacturing process that enables precise overlay of 8-inch to 6-inch wafers.

    CN116931381B