Preparation method and application of NH3-SCR catalyst

The catalyst is prepared by the ball milling method of Cu-SSZ-13 molecular sieve with rare earth and titanium raw materials, which solves the problems of low efficiency and poor anti-aging effect of the existing NH3-SCR catalyst at low temperatures, and achieves efficient and environmentally friendly catalytic reduction of nitrogen oxides. Effect.

CN118847201APending Publication Date: 2024-10-29LANZHOU UNIV +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410842440.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing NH3-SCR catalysts have problems such as narrow operating temperature window, V2O5 toxicity, low N2 selectivity, poor anti-aging effect, complex process and high cost, leading to the development of a vanadium-free, environmentally friendly SCR with excellent efficiency at low temperatures. Catalyst needs.

Method used

The catalyst is prepared by the ball milling method of Cu-SSZ-13 molecular sieve with rare earth and titanium raw materials. By mixing Cu-SSZ-13 molecular sieve, rare earth salt and titanium compound, it is prepared by agate ball milling, combined with the mechanochemical method, to produce a catalyst with excellent catalytic properties. NH3-SCR catalyst.

Benefits of technology

The catalyst is realized to have good catalytic effect and anti-aging performance at low temperature, long service life, simple process, environmental protection, and excellent SCR properties and structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847201A_ABST
    Figure CN118847201A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an NH3-SCR (Selective Catalytic Reduction) catalyst. The preparation method comprises the following steps: mixing raw materials for preparing the catalyst and carrying out ball milling; the raw materials comprise a Cu-SSZ-13 molecular sieve and a rare earth raw material, optionally a titanium raw material. The catalyst disclosed by the invention has a good low-temperature catalytic effect; the anti-aging effect is excellent, and the service life is relatively long; the catalyst is synthesized by adopting a mechanochemical method, and has the advantages of being green, simple to operate, rich in initiable structure change, uniform in product, easy to prepare on a large scale, high in surface activity of the product, capable of preparing structures which cannot be obtained by a conventional method and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a NH 3 -SCR catalyst and its preparation method and application. Background Art

[0002] Non-renewable fossil fuels are still the main energy source for thermal power plants, automobiles, cement and steel production. However, nitrogen oxides (NO, NO 2 、N 2 O and its derivatives) pollutants can cause acid rain, photochemical smog and ozone depletion. x Emissions are crucial to environmental protection. In order to prevent and control nitrogen oxide tail gas pollution, governments of various countries have formulated policies and regulations such as National VI or Euro VI to strictly limit diesel vehicle emissions. 3 -SCR) in NO x It has been widely used in the removal of NH 3 As a reducing agent, NO is converted into x Restored to harmless N 2 and H 2 O, the catalyst is NH 3 -The core of SCR technology, NH 3 Selective catalytic reduction of NO(NH 3 -SCR) has been proven to be a state-of-the-art NO x Removal technology. NH 3 -The core of SCR technology is to develop denitrification catalysts with high activity, strong selectivity, good hydrothermal stability and strong anti-poisoning ability. Denitrification catalysts are supported and solid solutions formed by several oxides. The carriers of supported catalysts include titanium oxide, aluminum oxide, molecular sieves and carbon materials.

[0003] Highly efficient NH 3 -SCR catalysts, such as Cu-exchanged SSZ-13 or SSZ-39 and various metal oxide catalysts, have made great progress. 3 or MoO 3 Promoted V 2 O 5 / TiO 2 In NH 3 -SCR has been widely commercialized, but still has the disadvantages of narrow operating temperature window and V 2 O 5 Toxicity and low N 2 The key defects are poor selectivity, poor anti-aging effect, complex process, high cost, etc. For these reasons, it is very necessary to develop a vanadium-free, environmentally friendly SCR catalyst with excellent efficiency at low temperature. Summary of the invention

[0004] In order to solve the above problems existing in the prior art, the present invention provides a NH 3 -Preparation method and application of SCR catalyst.

[0005] The first aspect of the present invention provides a NH 3 - A method for preparing an SCR catalyst comprises the following steps: mixing raw materials for preparing the catalyst and ball milling;

[0006] The raw materials include Cu-SSZ-13 molecular sieve and rare earth raw materials, optionally titanium raw materials.

[0007] According to some embodiments of the preparation method of the present invention, the rare earth raw material comprises a rare earth salt.

[0008] According to some embodiments of the preparation method of the present invention, the rare earth salt comprises one or more of rare earth acetylacetonate, rare earth nitrate and rare earth chloride.

[0009] According to some embodiments of the preparation method of the present invention, the rare earth salt comprises rare earth acetylacetonate.

[0010] According to some embodiments of the preparation method of the present invention, the rare earth element comprises one or more of cerium, lanthanum and samarium.

[0011] According to some embodiments of the preparation method of the present invention, the titanium raw material comprises a titanium compound and / or a titanium salt.

[0012] According to some embodiments of the preparation method of the present invention, the titanium compound comprises TiO 2 .

[0013] According to some embodiments of the preparation method of the present invention, the titanium salt comprises one or more of titanium acetylacetonate, titanium hydroxide and titanyl sulfate.

[0014] According to some embodiments of the preparation method of the present invention, the titanium salt comprises titanium acetylacetonate.

[0015] According to some embodiments of the preparation method of the present invention, the mass ratio of the Cu-SSZ-13 molecular sieve, the rare earth raw material and the titanium raw material is 10:(0.1-1):(0.1-1), for example, 10:0.1:0.1, 10:0.2:0.3, 10:0.3:0.5, 10:0.5:0.2, 10:0.5:0.5, 10:0.8:0.6, 10:0.7:0.9, 10:1:1.

[0016] According to some embodiments of the preparation method of the present invention, the mass ratio of the Cu-SSZ-13 molecular sieve, the rare earth raw material and the titanium raw material is 10: (0.1-0.5): (0.1-0.5).

[0017] According to some embodiments of the preparation method of the present invention, the mass ratio of the Cu-SSZ-13 molecular sieve, the rare earth raw material and the titanium raw material is 10:0.5:0.5.

[0018] According to some embodiments of the preparation method of the present invention, the mass ratio of the rare earth raw material to the titanium raw material is 1:(0.8-1.2), for example, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2.

[0019] According to some embodiments of the preparation method of the present invention, the raw material also includes a solvent.

[0020] According to some embodiments of the preparation method of the present invention, the solvent is selected from one or more of C1-C6 alcohol solvents, ether, acetone and chloroform, preferably ethanol.

[0021] According to some embodiments of the preparation method of the present invention, the mass ratio of the amount of the solvent to the Cu-SSZ-13 molecular sieve is (2-5):1, for example, 2:1, 3:1, 3.5:1, 4:1, 5:1.

[0022] According to some embodiments of the preparation method of the present invention, the ball milling is performed in the presence of ball milling media.

[0023] According to some embodiments of the preparation method of the present invention, the ball milling medium is selected from agate balls and / or zirconia balls, preferably agate balls.

[0024] According to some embodiments of the preparation method of the present invention, the particle size of the ball milling medium is 6-15 mm, for example, 6 mm, 8 mm, 10 mm, 12 mm, 13 mm, 15 mm.

[0025] According to some embodiments of the preparation method of the present invention, the ball milling medium is selected from one or more combinations of agate balls with a particle size of 6-15 mm, such as 6 mm, 8 mm, 10 mm, and 15 mm.

[0026] According to some embodiments of the preparation method of the present invention, the total mass ratio of the added amount of the ball milling medium to the Cu-SSZ-13 molecular sieve, rare earth raw material and titanium raw material is (5-7):1, for example 5:1, 6:1, 7:1.

[0027] According to some embodiments of the preparation method of the present invention, the rotation speed of the ball mill is 500-700 r / min, for example, 500 r / min, 600 r / min, 650 r / min, 700 r / min.

[0028] According to some embodiments of the preparation method of the present invention, the rotation speed of the ball mill is 550-650r / min.

[0029] According to some embodiments of the preparation method of the present invention, the ball milling time is 8-12 hours, for example, 8 hours, 10 hours, 11 hours, 12 hours.

[0030] According to some embodiments of the preparation method of the present invention, the ball milling device is a ball mill.

[0031] According to some embodiments of the preparation method of the present invention, the volume of the solvent is 1 / 10-1 / 15 of the volume of the ball mill tank of the ball mill.

[0032] According to some embodiments of the preparation method of the present invention, the preparation method further comprises: after the ball milling is completed, centrifuging, washing, drying and grinding the ball milled product in sequence to obtain the catalyst.

[0033] According to some embodiments of the preparation method of the present invention, the centrifugal rotation speed is 7000-9000 r / min, for example, 7000 r / min, 7500 r / min, 8000 r / min, 8500 r / min, 9000 r / min.

[0034] According to some embodiments of the preparation method of the present invention, the detergent used for washing includes a C1-C6 alcohol detergent and water.

[0035] According to some embodiments of the preparation method of the present invention, the detergent used for washing includes ethanol and deionized water.

[0036] According to some embodiments of the preparation method of the present invention, the washing comprises washing with ethanol and deionized water in sequence.

[0037] According to some embodiments of the preparation method of the present invention, the drying temperature is 50-70°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C.

[0038] According to some embodiments of the preparation method of the present invention, the drying time is 20-28 hours, for example, 20 hours, 22 hours, 25 hours, 26 hours, 28 hours.

[0039] According to some embodiments of the preparation method of the present invention, the grinding is carried out using an agate mortar.

[0040] According to some embodiments of the preparation method of the present invention, the particle size of the catalyst is 1-5 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm.

[0041] The second aspect of the present invention provides an application of the catalyst obtained by the preparation method described in the first aspect of the present invention in the catalytic reduction of nitrogen oxides.

[0042] The beneficial effects of the present invention include:

[0043] 1. The catalyst of the present invention has good low-temperature catalytic effect; it also has excellent anti-aging effect and a relatively long service life.

[0044] 2. The catalyst described in the present invention is synthesized by mechanochemical method, which has many advantages such as being green (using little or no solvent), simple operation, rich structural changes that can be induced, uniform products, high surface activity, easy large-scale preparation, and being able to prepare structures that cannot be obtained by conventional methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 NH described in Examples 1 to 4 of the present invention 3 - XRD pattern of SCR catalyst;

[0046] Figure 2 NH described in Examples 5 to 8 of the present invention 3 - XRD pattern of SCR catalyst;

[0047] Figure 3 NH described in Examples 9 to 11 and Comparative Example 1 of the present invention 3 - XRD pattern of SCR catalyst;

[0048] Figure 4 This is a SEM image of the Cu-SSZ-13 molecular sieve catalyst described in Comparative Example 1 of the present invention;

[0049] Figure 5 NH described in Example 10 of the present invention 3 - SEM image of SCR catalyst;

[0050] Figure 6 NH described in Example 1 of the present invention 3 - SEM image of SCR catalyst;

[0051] Figure 7 NH described in Example 11 of the present invention 3 - SEM image of SCR catalyst;

[0052] Figure 8This is a comparison chart of the SCR properties of the catalysts described in Example 1 of the present invention and Comparative Example 1;

[0053] Fig. 9 The catalysts described in Example 1 and Comparative Example 1 of the present invention catalyze NH 3 Transformation effect diagram;

[0054] Fig.10 This is a comparison chart of the SCR properties of the catalysts described in Example 2 of the present invention and Comparative Example 1;

[0055] Fig.11 This is a comparison chart of the SCR properties of the catalysts described in Example 1 and Example 5 of the present invention. DETAILED DESCRIPTION

[0056] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments and drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to constitute any limitation to the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concepts of the present disclosure. Such structures and technologies are also described in many publications.

[0057] Unless otherwise specified, the experimental methods used in the present invention are all conventional methods; the raw materials, reagents, instruments, etc. used are all available through commercial channels unless otherwise specified.

[0058] The Cu-SSZ-13 molecular sieve described in the embodiment of the present invention was purchased from Baidexin New Materials Co., Ltd.

[0059] Example 1

[0060] A cerium and titanium doped Cu-SSZ-13 molecular sieve NH 3 -SCR catalyst, the preparation method thereof comprises the following steps:

[0061] Take 10g Cu-SSZ-13 molecular sieve, 1g cerium acetylacetonate, 1g titanium dioxide, 40ml anhydrous ethanol, add to a ball mill with a volume of 500ml, add 72g agate balls with particle sizes of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding, and obtain a catalyst powder with a particle size of 1-5μm.

[0062] Example 2

[0063] A cerium-doped Cu-SSZ-13 molecular sieve with NH 3 -SCR catalyst, the preparation method thereof comprises the following steps:

[0064] Take 10g Cu-SSZ-13 molecular sieve, 1g cerium acetylacetonate, and 40ml anhydrous ethanol respectively, add them to a ball mill with a volume of 500ml, then add 66g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding, and obtain a catalyst powder with a particle size of 1-5μm.

[0065] Example 3

[0066] A lanthanum-doped Cu-SSZ-13 molecular sieve with NH 3 -SCR catalyst, the preparation method thereof comprises the following steps:

[0067] Take 10g Cu-SSZ-13 molecular sieve, 1.5g lanthanum acetylacetonate, and 40ml anhydrous ethanol respectively, add them to a ball mill with a volume of 500ml, then add 69g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven at a temperature of 60°C for 24h, and grind the dried catalyst product in an agate mortar to obtain a catalyst powder with a particle size of 1-5μm.

[0068] Example 4

[0069] A samarium-doped Cu-SSZ-13 molecular sieve NH 3 -SCR catalyst, the preparation method thereof comprises the following steps:

[0070] Take 10g Cu-SSZ-13 molecular sieve, 0.5g samarium acetylacetonate, and 40ml anhydrous ethanol respectively, add them to a ball mill with a volume of 500ml, then add 63g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding, and obtain a catalyst powder with a particle size of 1-5μm.

[0071] Example 5

[0072] The only difference from Example 1 is that cerium nitrate is used instead of cerium acetylacetonate.

[0073] Take 10g Cu-SSZ-13 molecular sieve, 1g cerium nitrate, 1g titanium dioxide, 40ml anhydrous ethanol, add to a ball mill with a volume of 500ml, add 72g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding, and obtain a catalyst powder with a particle size of 1-5μm.

[0074] Example 6

[0075] A Samarium and Titanium Doped Cu-SSZ-13 Molecular Sieve NH 3 -SCR catalyst, the preparation method thereof comprises the following steps:

[0076] Take 10g Cu-SSZ-13 molecular sieve, 1g samarium acetylacetonate, 1g titanium dioxide, and 40ml anhydrous ethanol respectively, add them to a ball mill with a volume of 500ml, then add 72g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding, and obtain a catalyst powder with a particle size of 1-5μm.

[0077] Example 7

[0078] A lanthanum and titanium doped Cu-SSZ-13 molecular sieve NH 3 -SCR catalyst, the preparation method thereof comprises the following steps:

[0079] Take 10g Cu-SSZ-13 molecular sieve, 1g lanthanum acetylacetonate, 1g titanium dioxide, 40ml anhydrous ethanol, add to a ball mill with a volume of 500ml, add 72g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding, and obtain a catalyst powder with a particle size of 1-5μm.

[0080] Example 8

[0081] The only difference from Example 1 is that the rotation speed of the ball mill is 800 r / min.

[0082] Take 10g Cu-SSZ-13 molecular sieve, 1g cerium acetylacetonate, 1g titanium dioxide, 40ml anhydrous ethanol, add to a ball mill with a volume of 500ml, add 72g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 800r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding to obtain a 0.5-5μm catalyst powder.

[0083] Example 9

[0084] The only difference from Example 1 is that the rotation speed of the ball mill is 200 r / min.

[0085] Take 10g Cu-SSZ-13 molecular sieve, 1g cerium acetylacetonate, 1g titanium dioxide, 40ml anhydrous ethanol, add to a ball mill with a volume of 500ml, add 72g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 10h at 200r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding to obtain a 2-10μm catalyst powder.

[0086] Example 10

[0087] The only difference from Example 1 is that the ball milling time is 1 h.

[0088] Take 10g Cu-SSZ-13 molecular sieve, 1g cerium acetylacetonate, 1g titanium dioxide, 40ml anhydrous ethanol, add to a ball mill with a volume of 500ml, add 72g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 1h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding to obtain a 2-10μm catalyst powder.

[0089] Embodiment 11

[0090] The only difference from Example 1 is that the ball milling time is 20 hours.

[0091] Take 10g Cu-SSZ-13 molecular sieve, 1g cerium acetylacetonate, 1g titanium dioxide, 40ml anhydrous ethanol, add to a ball mill with a volume of 500ml, add 72g agate balls with diameters of 6mm, 8mm, 10mm and 15mm and seal the ball mill, then install the ball mill on a planetary ball mill and grind for 20h at 600r / min. After grinding, centrifuge the liquid product at 8000r / min and wash it with ethanol and deionized water to obtain a catalyst product, put the catalyst product in an oven and dry it at 60°C for 24h, add the dried catalyst product to an agate mortar for grinding to obtain a 0.5-5μm catalyst powder.

[0092] Comparative Example 1

[0093] The catalyst described in Comparative Example 1 is a commercial Cu-SSZ-13 molecular sieve catalyst purchased from Weihai Baidexin New Materials Co., Ltd.

[0094] The catalysts described in Examples 1 to 11 and Comparative Example 1 of the present invention were analyzed by X-ray diffractometer, and the structures thereof were as follows: Figure 1-Figure 3 As shown:

[0095] from Figure 1-Figure 3 It can be seen that the phase composition of the catalysts described in Examples 1 to 11 is unchanged compared with the Cu-SSZ-13 molecular sieve described in Comparative Example 1, proving that rare earth and titanium are successfully incorporated into the lattice structure without generating new phases.

[0096] The structures of the catalysts described in Example 1, Example 10, Example 11 and Comparative Example 1 were analyzed and characterized using a scanning electron microscope. The results are as follows: Figure 4-7 As shown:

[0097] from Figure 4-7 It can be seen that the particle size of the synthesized doped Cu-SSZ-13 zeolite catalyst is smaller than that of the raw material Cu-SSZ-13 zeolite catalyst, and the corresponding specific surface area is increased; and the structure of the zeolite catalyst is diverse, such as round, square, and triangular; with the increase of ball milling time, the prepared zeolite particle size becomes smaller, the ball milling is not sufficient at 1 hour, and the doping elements cannot fully enter the zeolite; the ball milling is relatively sufficient at 10 hours, and the elements are doped into the zeolite; the ball milling time of 20 hours is too long, which seriously damages the structure of the zeolite and causes agglomeration, resulting in serious dealumination.

[0098] The catalysts described in Example 1, Example 2 and Comparative Example 1 were aged for 100 h at 600° C. and 10% water content (volume percentage) in air, and then SCR property tests were performed respectively.

[0099] The specific test method is: 500ppm NO + 500ppm NH 3 +10% O 2 (volume percentage), the rest is N 2 , volume space velocity 60000h -1 , react at a temperature of 100-550℃, and after the reaction is completed, measure the NO conversion rate and NH 3 The conversion rate of Figure 8-Figure 10 shown.

[0100] from Figures 8 to 10It can be seen that after cerium and titanium atoms are successfully incorporated into the lattice structure, the SCR activity of the catalyst can be effectively improved. The introduction of titanium improves the SCR performance of the catalyst, and the introduction of cerium improves the hydrothermal stability of the catalyst, thereby improving the conversion rate of nitrogen oxides and also improving the conversion of NH3.

[0101] The SCR (selective catalytic reduction technology) property test results of Example 1 and Example 5 are as follows: Fig.11 As shown:

[0102] Test method: 500 ppm NO + 500 ppm NH 3 +10% O 2 (volume percentage), the rest is N 2 , volume space velocity 60000h -1 , react at a temperature of 100-550℃, and after the reaction is completed, measure the NO conversion rate through a flue gas analyzer. The test results are as follows Fig.11 As shown:

[0103] from Fig.11 It can be seen that after using cerium nitrate instead of cerium acetylacetonate, the SCR properties of the catalyst in the two temperature ranges of 100-200°C and 350-550°C both decrease to a certain extent.

[0104] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing an NH3-SCR catalyst, comprising the following steps: Mixing raw materials for preparing the catalyst and performing ball milling; The raw materials include Cu-SSZ-13 molecular sieve and rare earth raw materials, optionally titanium raw materials.

2. The preparation method according to claim 1, characterized in that: The rare earth raw material comprises a rare earth salt, preferably, the rare earth salt comprises one or more of rare earth acetylacetonate, rare earth nitrate and rare earth chloride, more preferably rare earth acetylacetonate; And / or, the rare earth element comprises one or more of cerium, lanthanum and samarium; and / or, the titanium raw material comprises a titanium compound and / or a titanium salt; Preferably, the titanium compound comprises TiO2; Preferably, the titanium salt comprises one or more of titanium acetylacetonate, titanium hydroxide and titanyl sulfate, preferably titanium acetylacetonate.

3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the Cu-SSZ-13 molecular sieve, the rare earth raw material and the titanium raw material is 10:(0.1-1):(0.1-1); preferably 10:(0.1-0.5):(0.1-0.5), more preferably 10:0.5:0.5; And / or, the mass ratio of the rare earth raw material to the titanium raw material is 1:(0.8-1.2).

4. The preparation method according to any one of claims 1 to 3, characterized in that The raw material further comprises a solvent, preferably, the solvent is selected from one or more of C1-C6 alcohol solvents, ether, acetone and chloroform, preferably ethanol; And / or, the mass ratio of the amount of the solvent to the Cu-SSZ-13 molecular sieve is (2-5):

1.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The ball milling is carried out in the presence of a ball milling medium; Preferably, the ball milling media is selected from agate balls and / or zirconium oxide balls, preferably agate balls; Preferably, the particle size of the ball milling medium is 6-15 mm; Preferably, the ball milling media is selected from one or more combinations of agate balls with a particle size of 6-15 mm; And / or, the total mass ratio of the added amount of the ball milling medium to the Cu-SSZ-13 molecular sieve, the rare earth raw material and the titanium raw material is (5-7):

1.

6. The preparation method according to any one of claims 4 to 5, characterized in that: The rotation speed of the ball mill is 500-700r / min, preferably 550-650r / min; And / or, the ball milling time is 8-12h; And / or, the ball milling is carried out using a ball mill; And / or, the volume of the solvent is 1 / 10-1 / 15 of the volume of the ball mill tank of the ball mill.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method further comprises: after the ball milling is completed, the ball milling product is subjected to centrifugation, washing, drying and grinding treatment in sequence to obtain the catalyst.

8. The preparation method according to claim 7, characterized in that: The centrifugal speed is 7000-9000r / min; And / or, the washing detergent comprises a C1-C6 alcohol detergent and water, preferably ethanol and deionized water; More preferably, the washing comprises washing with ethanol and deionized water in sequence.

9. The preparation method according to claim 7 or 8, characterized in that: The drying temperature is 50-70°C; and / or the drying time is 20-28h; And / or, the grinding is performed using an agate mortar; And / or, the particle size of the catalyst is 1-5 μm.

10. Use of the catalyst obtained by the preparation method according to any one of claims 1 to 9 in the catalytic reduction of nitrogen oxides.

Citation Information

Patent Citations

  • Rare-earth-based SCR denitration catalyst and preparation method thereof

    CN106423139A

  • Rare earth metal modified Cu-SSZ-13 molecular sieve and preparation method and application thereof

    CN111135860A

  • Molecular sieve SCR catalyst and preparation method thereof

    CN113318780A

  • NH3-SCR (selective catalytic reduction) catalyst as well as preparation method and application thereof

    CN116510773A

  • Preparation method and application of Cu-SSZ-13 composite catalyst loaded with rare earth metal oxide or transition metal oxide

    CN116550376A