Efficient waste gas treatment method

Through the pretreatment of dust slurry of calcined arc furnace and the deep treatment of carbon-loaded phosphomolybdate materials for co-doping of nitrogen and sulfur in carbon-loaded phosphomolybic acid, combined with alkaline absorption, the problems of catalyst poisoning and inactivation and high energy consumption in the exhaust gas treatment of carbon black production are solved, and the problem of catalyst poisoning and inactivation and high energy consumption are achieved. It has efficient desulfurization and denitrification effect and reduces treatment costs.

CN118892729APending Publication Date: 2024-11-05青州市博奥炭黑有限责任公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410928351.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing carbon black production exhaust gas treatment methods have problems such as catalyst poisoning and inactivation, high energy consumption and high cost, and the MnOx/CePO4 material is expensive and the catalytic oxidation treatment temperature is high.

Method used

The carbon black production exhaust gas is pretreated by calcined arc furnace dust slurry, copper-molybdenum nitrogen and sulfur co-doped carbon-loaded phosphomolybic acid material is used for in-depth treatment, and desulfurization and denitrogenation is carried out through alkali absorption, improving the desulfurization and denitrification efficiency and reducing costs.

Benefits of technology

The desulfurization efficiency of more than 99% and the detonation efficiency of more than 98% is achieved, which reduces the treatment cost and improves the activity and redox activity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004938901650000141
    Figure BDA0004938901650000141
  • Figure BDA0004938901650000151
    Figure BDA0004938901650000151
Patent Text Reader

Abstract

The invention discloses an efficient waste gas treatment method which comprises the following steps: sequentially feeding carbon black production tail gas into a pretreatment tower, and treating the tail gas by calcining electric arc furnace dust slurry; the tail gas enters a deep treatment tower and is subjected to deep treatment under catalysis of a desulfurization and denitrification catalyst, and the desulfurization and denitrification catalyst takes a copper-modified nitrogen-sulfur co-doped carbon material as a carrier and takes phosphomolybdic acid as an active component; and the deeply treated tail gas enters an absorption tower for absorption treatment. According to the method, the carbon black production tail gas is pretreated by adopting the calcined electric arc furnace dust slurry, then the tail gas is deeply treated by adopting the copper-modified nitrogen-sulfur co-doped carbon-loaded phosphomolybdic acid material, and finally the tail gas is absorbed by adopting the alkali liquor, so that the desulfurization and denitrification efficiency is high, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste gas treatment, and in particular to a high-efficiency waste gas treatment method. Background Art

[0002] Carbon black is a black powdery substance formed by incomplete combustion or pyrolysis of hydrocarbons in the gas phase under strictly controlled process conditions. Its main component is carbon and contains a small amount of oxygen, hydrogen, sulfur and other elements. Carbon black particles are approximately spherical, with a particle size between 10 and 500 μm. In rubber processing, carbon black is added to rubber through mixing as a reinforcing agent and filler.

[0003] At present, the oil furnace method is the most efficient and economically beneficial carbon black production method. The output of oil furnace black has accounted for 70% to 90% of the total carbon black. When the oil furnace method is used to produce carbon black, a large amount of tail gas containing nitrogen oxides and sulfur oxides will be generated. If the above tail gas is not treated in time, it will pollute the atmosphere. Selective catalytic reduction is the main method for treating tail gas containing nitrogen oxides and sulfur oxides. The patent with application number 202211590504.4 provides a tail gas treatment method for producing carbon black, including: S1, aliphatic saturated hydrocarbons are cracked in a high-temperature combustion gas flow to obtain carbon black flue gas; S2, the carbon black flue gas is cooled once, and then cooled twice, and then the carbon black and tail gas are separated; S3, the tail gas is treated with a selective catalytic reducing agent, and then the tail gas is used for carbon black drying treatment, and then the tail gas is successively desulfurized and dusted, and the tail gas is discharged after passing the test; the selective catalytic reducing agent is MnOx / CePO4. Although the above method can effectively remove pollutants in tail gas to a certain extent, harmful substances such as sulfide still exist in the tail gas, which will cause the catalyst to be poisoned and deactivated, greatly affecting the denitration efficiency and the service life of the catalyst. In addition, the above MnOx / CePO4 material is expensive, and the temperature required for catalytic oxidation treatment of tail gas is relatively high, which greatly increases energy consumption. Based on the above problems, it is necessary to provide a method with high catalytic efficiency and low cost to treat carbon black production tail gas. Summary of the invention

[0004] The technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, an efficient method for treating waste gas is provided. The present invention firstly adopts calcined arc furnace dust slurry to pretreat the tail gas from carbon black production, then adopts copper-modified nitrogen-sulfur co-doped carbon-loaded phosphomolybdic acid material to deeply treat the tail gas, and finally adopts alkaline solution to absorb the tail gas, so that the desulfurization and denitrification efficiency is high and the cost is low.

[0005] In order to solve the above technical problems, the technical solution of the present invention is:

[0006] An efficient method for treating waste gas comprises the following steps:

[0007] S1: calcining the electric arc furnace dust in an oxygen atmosphere at 750-850° C. for 1-2 hours, adding the calcined electric arc furnace dust into water and stirring to prepare a calcined electric arc furnace dust slurry with a solid content of 5-10wt%;

[0008] S2: The tail gas from carbon black production is sequentially fed into a pretreatment tower and treated with calcined arc furnace dust slurry;

[0009] S3: the tail gas enters a deep treatment tower and is deeply treated under the catalysis of a desulfurization and denitration catalyst, wherein the desulfurization and denitration catalyst is obtained by using a copper-modified nitrogen-sulfur co-doped carbon material as a carrier and loaded with phosphomolybdic acid;

[0010] S4: The tail gas after deep treatment enters the absorption tower for absorption treatment.

[0011] Preferably, in step S1, the heating rate during the calcination treatment is 8-10°C / min.

[0012] Preferably, in step S2, when a pretreatment tower is used for treatment, the process also includes the step of introducing oxygen into the pretreatment tower, wherein the carbon black production tail gas is premixed with oxygen to obtain a mixed gas, and preheating treatment is performed, and the preheating temperature is 50-60°C; and / or the oxygen content in the mixed gas is 10-20v / v%; and / or the temperature during pretreatment is 50-60°C; and / or during pretreatment, the amount ratio of the calcined arc furnace dust slurry to the mixed gas is (5-10)g:1Nm3, and the introduction rate of the mixed gas is 300-400ml / min.

[0013] Preferably, in step S3, the method for preparing the desulfurization and denitration catalyst comprises the following steps:

[0014] 1. Using activated carbon as a matrix and thiourea as a doping raw material, calcining is performed in a nitrogen atmosphere to obtain a nitrogen-sulfur co-doped carbon material; the nitrogen-sulfur co-doped carbon material is dispersed in a solvent, and then a copper source and trimesic acid are added, mixed evenly, and then placed in a reactor for reaction, and the solid obtained by the reaction is dried and calcined to obtain a copper-modified nitrogen-sulfur co-doped carbon material;

[0015] 2. After dispersing the copper-modified nitrogen-sulfur co-doped carbon material, add hydrochloric acid solution to adjust the pH, then add phosphomolybdic acid dispersion, perform ultrasonic treatment, and then dry to obtain a desulfurization and denitrification catalyst.

[0016] Preferably, in step one, when preparing the nitrogen-sulfur co-doped carbon material, the mass ratio of thiourea to activated carbon is (0.5-1.5):1; and / or the temperature during calcination treatment is 490-510°C; and / or the heating rate during calcination treatment is 5-10°C / min; and / or the calcination treatment time is 1-2h; and / or the nitrogen flow rate during calcination treatment is 100-120ml / min.

[0017] Preferably, in step one, the copper source is copper nitrate trihydrate; and / or the mass ratio of the copper source, trimesic acid, and nitrogen-sulfur co-doped carbon material is 2.1:(1-2):(2-2.5); and / or the solvent is a mixture of DMF, water and ethanol, and the volume ratio of DMF, water and ethanol is 1:1:1; and / or the reaction temperature is 80-90°C and the reaction time is 20-30h.

[0018] Preferably, in step one, the calcination atmosphere during the preparation of the copper-modified nitrogen-sulfur co-doped carbon material is a nitrogen atmosphere, and the nitrogen flow rate during calcination is 100-120 ml / min; and / or the calcination temperature is 550-600°C, the calcination time is 1-2h; and / or the heating rate during calcination is 5-10°C / min.

[0019] Preferably, in step 2, the concentration of the hydrochloric acid solution is 1-1.5 mol / L, and the pH is adjusted to 3-3.5; and / or the concentration of the phosphomolybdic acid dispersion is 0.05-0.1 g / ml; and / or the mass ratio of the copper-modified nitrogen-sulfur co-doped carbon material to the phosphomolybdic acid is 1:(0.1-0.5).

[0020] Preferably, in step S3, the deep treatment also includes the step of mixing the tail gas discharged from the pretreatment tower with oxygen, and the concentration of oxygen in the mixed gas is 5-10v / v%; and / or the weight hourly space velocity of the gas during the deep treatment is (4900-5000) ml·h-1·g-1; and / or the temperature during the deep treatment is 40-60°C.

[0021] Preferably, an efficient method for treating waste gas also includes the following steps: the exhaust gas after absorption treatment is tested by a flue gas analyzer to detect the concentrations of nitrogen oxides and sulfur oxides in the exhaust gas. If the concentrations of nitrogen oxides and sulfur oxides meet the emission standards, they are directly discharged, otherwise the exhaust gas continues to be absorbed.

[0022] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0023] In order to reduce the treatment cost of carbon black production tail gas, the present invention uses waste electric arc furnace dust as a treatment agent. The electric arc furnace dust contains a large amount of zinc oxide and zinc ferrite. Zinc oxide and zinc ferrite are used as desulfurization active phases to effectively remove sulfur oxides in the tail gas. In order to improve the treatment effect, the present invention also calcines the electric arc furnace dust. By effectively controlling the calcination conditions, the crystallinity of zinc oxide and zinc ferrite is effectively improved while ensuring a high specific surface area of ​​the electric arc furnace dust, thereby improving the desulfurization and denitrification efficiency.

[0024] The present invention also uses low-cost activated carbon as raw material. The activated carbon has developed pores, a large specific surface area and abundant surface functional groups, and can effectively adsorb sulfur oxides and nitrogen oxides in exhaust gas. In order to improve the low-temperature catalytic performance of activated carbon, the present invention uses thiourea as a doping raw material and co-dopes the activated carbon with nitrogen and sulfur, which promotes the formation of oxygen vacancies on the catalyst surface, increases the acidic sites and oxygen adsorption capacity of the catalyst, and further improves the low-temperature catalytic performance of the catalyst and improves the desulfurization and denitrification efficiency.

[0025] In addition, in order to further improve the desulfurization and denitrification efficiency, the present invention in situ grows Cu-MOF on the surface of nitrogen-sulfur co-doped carbon material, and then calcines under certain conditions to promote the decomposition of Cu-MOF, thereby modifying copper nanoparticles on the surface of nitrogen-sulfur co-doped carbon material, improving the active center of the catalyst, and further improving the desulfurization and denitrification performance of the catalyst. Finally, the present invention also loads phosphomolybdic acid with copper-modified nitrogen-sulfur doped carbon material, and phosphomolybdic acid has high catalytic activity and redox activity, which further improves the desulfurization and denitrification efficiency of the catalyst. The method provided by the present invention achieves a desulfurization efficiency of more than 99% and a denitrification efficiency of more than 98%. DETAILED DESCRIPTION

[0026] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0027] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0028] In order to effectively treat the tail gas in the production of carbon black, the present invention provides an efficient method for treating the waste gas, comprising the following steps:

[0029] S1: The tail gas from carbon black production enters the pretreatment tower in sequence, and the tail gas is treated with calcined arc furnace dust slurry;

[0030] S2: The tail gas enters a deep treatment tower and is deeply treated under the catalysis of a desulfurization and denitration catalyst, wherein the desulfurization and denitration catalyst uses a copper-modified nitrogen-sulfur co-doped carbon material as a carrier and phosphomolybdic acid as an active component;

[0031] S3: The tail gas after deep treatment enters the absorption tower for absorption treatment.

[0032] Regarding step S1:

[0033] In the present invention, the solid content of the calcined arc furnace dust slurry is 5-10wt%. Further, the solid content of the calcined arc furnace dust slurry may preferably be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, but not limited thereto.

[0034] Electric arc furnace dust is a by-product of the electric arc furnace steelmaking process. Its main components are zinc oxide and zinc ferrite, which can be used as desulfurization active phases to pretreat carbon black production exhaust gas.

[0035] In the present invention, the present invention also provides a method for preparing calcined arc furnace dust slurry, specifically:

[0036] Calcine the electric arc furnace dust;

[0037] The calcined electric arc furnace dust is added into water and stirred to prepare the calcined electric arc furnace dust slurry.

[0038] In the present invention, the atmosphere during the calcination treatment is oxygen. In the oxygen atmosphere, the zinc oxide and zinc ferrite in the calcined electric arc furnace dust have higher crystallinity, thereby improving the desulfurization performance of the electric arc furnace dust.

[0039] In the present invention, the temperature during the calcination treatment is 750-850° C. Further, the temperature during the calcination treatment may preferably be 750° C., 760° C., 770° C., 780° C., 790° C., 800° C., 810° C., 820° C., 830° C., 840° C., 850° C., but is not limited thereto.

[0040] In the present invention, the calcination time is 1-2 hours. Further, the calcination time is preferably 1 hour, 1.5 hours, or 2 hours.

[0041] With the increase of calcination temperature and the extension of calcination time, the crystallinity of zinc oxide and zinc ferrite in electric arc furnace dust is significantly improved, but the calcination temperature is too high and the calcination time is too long, and the desulfurization performance of the obtained calcined electric arc furnace dust is reduced. This is mainly because, if the calcination time is too long, the ferroferric oxide in the electric arc furnace dust will be converted into iron oxide under an oxygen atmosphere, and iron oxide will react with zinc oxide to form zinc ferrite, and the desulfurization performance of zinc ferrite is not as good as zinc oxide. In addition, if the calcination temperature is too high or the calcination time is too long, the crystallinity of zinc oxide and zinc ferrite will be too high, resulting in a smooth surface of the material, which is not conducive to the contact between the tail gas and the calcined electric arc furnace dust slurry, thereby causing the desulfurization performance to decrease. Therefore, it is necessary to strictly control the calcination temperature and calcination time during the specific operation.

[0042] In the present invention, the heating rate during the calcination treatment is 8-10°C / min. Further, the heating rate during the calcination treatment may be specifically preferably 8°C / min, 8.5°C / min, 9°C / min, 9.5°C / min, 10°C / min, but is not limited thereto.

[0043] The heating rate when calcining arc furnace dust has a significant effect on the crystallinity of zinc oxide and zinc ferrite. A slow heating rate will improve the integrity of the crystal to a certain extent, thereby improving the crystallinity of zinc oxide and zinc ferrite. However, if the heating rate is too slow, it will not only reduce the calcination efficiency, but also cause the product grains to be too large, and even cause an increase in defects in the crystal structure, resulting in the crystallinity of zinc oxide and zinc ferrite not being significantly improved, or even possibly decreasing. Therefore, it is necessary to select a suitable heating rate to ensure the crystallinity of zinc oxide and zinc ferrite.

[0044] In the present invention, when a pretreatment tower is used for treatment, the step of introducing oxygen into the pretreatment tower is also included. Specifically, during pretreatment, the carbon black production tail gas is first premixed with oxygen and preheated at a temperature of 50-60°C.

[0045] In the present invention, the oxygen content in the mixed gas is 10-20 v / v%. The specific oxygen content may be preferably 10 v / v%, 15 v / v%, 20 v / v%, but is not limited thereto.

[0046] The higher the oxygen content in the mixed gas, the higher the desulfurization efficiency. This is mainly because the presence of oxygen molecules promotes the conversion of sulfur dioxide into sulfate during wet desulfurization. However, when the dissolved oxygen required by the reaction system is saturated, the oxygen content in the mixed gas continues to increase, and the desulfurization efficiency of the calcined arc furnace dust slurry no longer increases. Therefore, based on desulfurization performance and economic cost considerations, the oxygen content in the mixed gas is controlled to be 10-20v / v%.

[0047] In the present invention, the temperature during the pretreatment is 50-60° C. Specifically, the temperature of the pretreatment is preferably 50° C., 55° C., or 60° C., but is not limited thereto.

[0048] As the pretreatment temperature increases, the contact efficiency between the gas and the calcined arc furnace dust also increases, and the desulfurization efficiency improves. However, if the pretreatment temperature is too high, the dissolved oxygen content in the reaction system will be reduced, thereby reducing the desulfurization efficiency. Therefore, it is necessary to reasonably control the pretreatment temperature.

[0049] In the present invention, the ratio of the calcined arc furnace dust slurry to the mixed gas during pretreatment is (5-10) g: 1 Nm 3 , the introduction rate of the mixed gas is 300-400ml / min. Specifically, the ratio of the calcined arc furnace dust slurry to the tail gas during pretreatment is 5g:1Nm3 , 6g: 1Nm 3 , 7g: 1Nm 3 , 8g: 1Nm 3 , 9g: 1Nm 3 , 10g: 1Nm 3 , but not limited thereto. The tail gas introduction rate is preferably 300ml / min, 350ml / min, 400ml / min, but not limited thereto. In the pretreatment, if the amount of calcined arc furnace dust slurry is too small, the pretreatment efficiency is not good, but if the amount is too large, it will cause a waste of resources.

[0050] In the above pretreatment process, zinc oxide in the calcined arc furnace dust is used as the main desulfurization active phase, zinc ferrite is used as the auxiliary desulfurization active phase, and zinc oxide reacts with sulfur dioxide in the tail gas of carbon black production to produce sulfate ions and zinc ions, resulting in a decrease in the pH of the slurry, thereby leaching trivalent iron ions. The leached iron ions can oxidize tetravalent sulfur to hexavalent sulfur, and the reduced divalent iron ions are oxidized to trivalent iron ions under the action of dissolved oxygen. Such a chain reaction greatly improves the desulfurization effect of the process. The desulfurization slag produced in the pretreatment process contains a large amount of zinc ferrite, which can be recycled and used as a photo-Fenton catalyst.

[0051] Regarding step S2:

[0052] In the present invention, in step S2, the method for preparing the desulfurization and denitration catalyst comprises the following steps:

[0053] (1) using activated carbon as a matrix and thiourea as a sulfur source, calcining in a nitrogen atmosphere to obtain a nitrogen-sulfur co-doped carbon material;

[0054] (2) dispersing the nitrogen-sulfur co-doped carbon material in a solvent, then adding a copper source and trimesic acid, mixing them evenly and placing them in a reactor for reaction, drying the solid obtained by the reaction and calcining it to obtain a copper-modified nitrogen-sulfur co-doped carbon material;

[0055] (3) After the copper-modified nitrogen-sulfur co-doped carbon material is dispersed, a hydrochloric acid solution is added to adjust the pH, and then a phosphomolybdic acid dispersion is added, ultrasonically treated, and then dried to obtain a desulfurization and denitrification catalyst.

[0056] In the present invention, the mass ratio of thiourea to activated carbon is (0.5-1.5): 1. Specifically, the mass ratio of thiourea to activated carbon is preferably 0.5: 1, 0.7: 1, 0.9: 1, 1.1: 1, 1.3: 1, 1.5: 1, but not limited thereto. The present invention uses thiourea as a doping raw material to achieve nitrogen-sulfur co-doping of activated carbon materials. The amount of thiourea added determines the amount of nitrogen-sulfur doping. Within a certain range, as the amount of nitrogen-sulfur doping increases, the medium-strong acid center of the desulfurization and denitration catalyst will be greatly increased, and it will be more conducive to the increase in the proportion of surface oxygen in the catalyst, thereby improving the catalytic activity of the catalyst. Moreover, the surface of the material after nitrogen-sulfur co-doping will become rough and porous, which is more conducive to the adsorption of gas during the treatment process. However, if the doping amount is too much, the penetration of nitrogen and sulfur substances will seriously damage the integrity of the pores of the activated carbon matrix, thereby causing partial blockage of the pores, thereby reducing the specific surface area of ​​the activated carbon, which is not conducive to the contact between the gas and the surface of the desulfurization and denitration catalyst.

[0057] In the present invention, the temperature during calcination is 490-510°C, and the calcination time is 1-2h. Specifically, the temperature during calcination is preferably 490°C, 495°C, 500°C, 505°C, 510°C, but not limited thereto; the calcination time is preferably 1h, 1.5h, 2h, but not limited thereto.

[0058] In the present invention, the heating rate during the calcination treatment is 5-10°C / min. Specifically, the heating rate during the calcination treatment is preferably 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, but is not limited thereto.

[0059] In the present invention, the nitrogen flow rate is 100-120 ml / min. Specifically, the nitrogen flow rate is preferably 100 ml / min, 105 ml / min, 110 ml / min, 115 ml / min, 120 ml / min, but is not limited thereto.

[0060] In the above calcination process, the calcination temperature, heating rate, nitrogen flow rate and calcination time will have a certain influence on the performance of the desulfurization and denitration catalyst. If the calcination temperature is too low, the material will not be fully converted, so the doping effect is not obvious, and if the calcination temperature is too high, it will cause sintering between the particles, resulting in a decrease in the porosity of the material, and reduce the specific surface area and adsorption performance of the material. For the heating rate, a higher heating rate will shorten the calcination time, but a heating rate that is too fast will cause uneven heating of the material, thereby generating local internal stress, which will affect the performance of the material. For the calcination time, as the calcination time increases, the crystal growth and stable lattice structure of the material will be promoted, but if the calcination time is too long, it will cause the material to burn, affect the microstructure and specific surface area of ​​the material, and increase energy consumption. For the nitrogen flow rate, as the nitrogen flow rate increases, the nitrogen doping amount in the material will increase, but if the nitrogen flow rate is too large, the integrity of the activated carbon matrix pores will be destroyed, resulting in partial blockage of the pores, thereby reducing the specific surface area of ​​the activated carbon, which is not conducive to the contact between the gas and the surface of the desulfurization and denitration catalyst. Therefore, the calcination conditions need to be strictly controlled when preparing nitrogen-sulfur co-doped carbon materials.

[0061] In some embodiments, in step (2), the solvent is a mixture of DMF, water and ethanol, and the volume ratio of DMF, water and ethanol is 1:1:1.

[0062] In the present invention, the copper source is copper nitrate trihydrate, and the mass ratio of copper nitrate trihydrate, trimesic acid, and nitrogen-sulfur co-doped carbon material is 2.1:(1-2):(2-2.5). Specifically, the mass ratio of copper nitrate trihydrate, trimesic acid, and nitrogen-sulfur co-doped carbon material is preferably 2.1:1:2, 2.1:1:2.1, 2.1:1:2.2, 2.1:1:2.3, 2.1:1:2.4, 2.1:1:2.5, but is not limited thereto.

[0063] In the present invention, in step (2), the reaction temperature is 80-90°C and the reaction time is 20-30h. Specifically, the reaction temperature is preferably 80°C, 85°C, 90°C, but not limited thereto. The reaction time is preferably 20h, 22h, 24h, 26h, 28h, 30h, but not limited thereto.

[0064] In the present invention, in step (2), the calcination atmosphere is a nitrogen atmosphere, and the nitrogen flow rate during calcination is 100-120 ml / min. Specifically, the nitrogen flow rate during calcination is preferably 100 ml / min, 105 ml / min, 110 ml / min, 115 ml / min, 120 ml / min, but is not limited thereto.

[0065] In the present invention, the calcination temperature is 550-600° C. Specifically, the calcination temperature is preferably 550° C., 550-600° C., 560° C., 570° C., 580° C., 590° C., but is not limited thereto.

[0066] In the present invention, the calcination time is 1-2 hours. Specifically, the calcination time is preferably 60 minutes, 80 minutes, 100 minutes, 120 minutes, but is not limited thereto.

[0067] In the present invention, the heating rate during calcination is 5-10°C / min. Specifically, the heating rate during calcination is preferably 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, but is not limited thereto.

[0068] The present invention in-situ grows Cu-MOF material on the surface of nitrogen-sulfur co-doped carbon material, and then calcines it under certain conditions, and the Cu-MOF is pyrolyzed to generate uniformly dispersed copper nanoparticles. In the above process, for the copper modification amount, within a certain range, as the copper modification amount increases, the desulfurization and denitrification activity of the catalyst is greatly increased, which mainly depends on the high activity surface of the copper nanoparticles, but if the copper modification amount is too much, it will cause the agglomeration of copper particles, thereby reducing the active center of the catalyst, and the catalytic activity of the catalyst will also be reduced. For the calcination temperature, within a certain range, as the calcination temperature increases, it is more conducive to the decomposition of the Cu-MOF material, thereby increasing the specific surface area of ​​the catalyst and the increase of active adsorption sites, but if the calcination temperature is too high, it will cause the agglomeration of copper nanoparticles on the surface of the nitrogen-sulfur co-doped carbon material.

[0069] In the present invention, in step (3), the concentration of the hydrochloric acid solution is 1-1.5 mol / L, and the pH is adjusted to 3-3.5. Specifically, the concentration of the hydrochloric acid solution is preferably 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, but is not limited thereto.

[0070] In the present invention, the concentration of the phosphomolybdic acid dispersion is 0.05-0.1 g / ml. Specifically, the concentration of the phosphomolybdic acid dispersion is preferably 0.05 g / ml, 0.06 g / ml, 0.07 g / ml, 0.08 g / ml, 0.09 g / ml, 0.1 g / ml, but is not limited thereto.

[0071] In the present invention, the mass ratio of the copper-modified nitrogen-sulfur co-doped carbon material to the phosphomolybdic acid is 1:(0.1-0.5). Specifically, the mass ratio of the copper-modified nitrogen-sulfur co-doped carbon material to the phosphomolybdic acid may be preferably 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, but is not limited thereto.

[0072] Phosphomolybdic acid has high catalytic activity and redox activity. In order to better achieve the separation of phosphomolybdic acid, the present invention uses copper-modified nitrogen-sulfur co-doped carbon material as a carrier to achieve the loading of phosphomolybdic acid. As the loading amount of phosphomolybdic acid increases, the catalytic activity of the catalyst is also significantly improved, but too much phosphomolybdic acid loading will not only increase the cost of the catalyst, but also lead to excessive blockage of active sites on the catalyst surface, limiting the contact between gas molecules and active sites, which will reduce the catalytic activity of the catalyst, thereby weakening the effect of desulfurization and denitration reactions.

[0073] In the present invention, in step S2, the deep treatment further includes the step of mixing the tail gas discharged from the pretreatment tower with oxygen. Further, the concentration of oxygen in the mixed gas is 5-10 v / v%; further, the weight hourly space velocity of the gas during the deep treatment is (4900-5000) ml·h -1 ·g -1 , the temperature is 40-60°C. Specifically, the concentration of oxygen in the mixed gas is preferably 5v / v%, 6v / v%, 7v / v%, 8v / v%, 9v / v%, 10v / v%; the weight hourly space velocity of the gas during deep treatment is preferably 4900ml·h -1 ·g -1 、4950ml·h -1 ·g -1 、5000ml·h -1 ·g -1 The temperature during deep treatment is preferably 40°C, 45°C, 50°C, 55°C, or 60°C, but is not limited thereto.

[0074] In the present invention, in step S3, the absorption liquid used in the absorption treatment is an alkaline solution, which is a sodium hydroxide solution with a concentration of 0.1-0.5 mol / L. In the case of spray absorption, the spray conditions are not specifically limited, and the spray method commonly used in the art can be used.

[0075] In the present invention, the desulfurization and denitrification method also includes the following steps: the exhaust gas after absorption treatment is tested by a flue gas analyzer to detect the concentration of nitrogen oxides and sulfur oxides in the exhaust gas. If the concentration of nitrogen oxides and sulfur oxides reaches the emission standard, they are directly discharged, otherwise the exhaust gas continues to be absorbed.

[0076] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0077] In the following examples, the electric arc furnace dust comes from Shandong Luli Steel Co., Ltd., and the activated carbon comes from Fuchen (Tianjin) Chemical Reagent Co., Ltd., and its average particle size is 40-60 mesh. Other reagents are commercially available unless otherwise specified. The carbon black production tail gas in the following examples and comparative examples is the tail gas generated during the production of carbon black by Qingzhou Bio Carbon Black Co., Ltd.

[0078] Example 1

[0079] An efficient method for treating waste gas comprises the following steps:

[0080] 1. Preparation of calcined arc furnace dust slurry:

[0081] The electric arc furnace dust is placed in a high-temperature tube furnace, and heated to 800° C. at a heating rate of 10° C. / min for calcination for 2 hours under an oxygen atmosphere to obtain calcined electric arc furnace dust; the calcined electric arc furnace dust is mixed with water and stirred evenly to obtain a calcined electric arc furnace dust slurry with a solid content of 10 wt%;

[0082] 2. Preparation of desulfurization and denitrification catalysts:

[0083] 1 g of activated carbon and 1.2 g of thiourea were added to 100 ml of ultrapure water, stirred and mixed at room temperature for 10 h, and then dried. The obtained solid was placed in a high-temperature tube furnace, heated to 500 ° C at a rate of 10 ° C / min under a nitrogen atmosphere, and calcined for 1 h. During the calcination process, the nitrogen flow rate was controlled to be 100 ml / min. After the calcination, the furnace was cooled to room temperature to obtain a nitrogen-sulfur co-doped carbon material;

[0084] 2.1 g of nitrogen-sulfur co-doped carbon material was dispersed in a mixed solvent consisting of 20 ml of DMF, 20 ml of water and 20 ml of ethanol, and then 2.1 g of copper nitrate trihydrate and 1 g of trimesic acid were added, mixed evenly and placed in a reactor, reacted at 85° C. for 20 h, the solid obtained by the reaction was dried and placed in a high-temperature tubular furnace, heated to 600° C. at a heating rate of 10° C. / min under a nitrogen atmosphere, and calcined for 2 h. The nitrogen flow rate during the calcination process was controlled to be 100 ml / min. After the calcination was completed, the copper-modified nitrogen-sulfur co-doped carbon material was cooled to room temperature with the furnace to obtain a copper-modified nitrogen-sulfur co-doped carbon material;

[0085] After dispersing 1g of copper-modified nitrogen-sulfur co-doped carbon material in 20ml of deionized water, a 1mol / L hydrochloric acid solution was added to adjust the pH to 3.0, and then 5ml of 0.08g / ml phosphomolybdic acid dispersion was added, and ultrasonic treatment was performed at 500W for 1h, and then dried to obtain a desulfurization and denitrification catalyst;

[0086] 3. Preprocessing:

[0087] The carbon black production tail gas and oxygen are premixed to obtain a mixed gas, and the mixed gas is preheated to 55°C, and the oxygen content in the mixed gas is controlled to be 15v / v%; the mixed gas is introduced into the lower part of the pretreatment tower filled with electric arc furnace dust slurry at a speed of 300ml / min, and pretreated at 55°C. During the pretreatment, the amount ratio of calcined electric arc furnace dust slurry to the mixed gas is 8g:1Nm 3 ;

[0088] 4. Deep processing:

[0089] The above-mentioned desulfurization and denitration catalyst is loaded into the deep treatment tower. The gas discharged from the top of the pretreatment tower is mixed with oxygen and then enters from the bottom of the deep treatment tower. The weight hourly space velocity is 5000 ml·h -1 ·g -1 , the oxygen concentration was controlled at 5v / v%, and deep treatment was performed at 50°C;

[0090] 5. Absorption treatment:

[0091] The gas discharged from the top of the deep treatment tower enters the lower part of the absorption tower. At the same time, a sodium hydroxide solution with a concentration of 0.5 mol / L is added to the upper part of the absorption tower for spraying treatment. The exhaust gas discharged from the top of the absorption tower is tested by a flue gas analyzer to detect the concentration of nitrogen oxides and sulfur oxides in the exhaust gas. If the concentration of nitrogen oxides and sulfur oxides reaches the emission standard, they are directly discharged. Otherwise, the exhaust gas re-enters the absorption tower for further absorption treatment.

[0092] Example 2

[0093] The difference between this embodiment and embodiment 1 is that when preparing the calcined arc furnace dust slurry, the calcination temperature is 750° C., and the other conditions are the same as those in embodiment 1.

[0094] Example 3

[0095] The difference between this embodiment and embodiment 1 is that the temperature during pretreatment is 60° C., and other conditions are the same as those in embodiment 1.

[0096] Example 4

[0097] The difference between this embodiment and embodiment 1 is that the oxygen content in the mixed gas during pretreatment is 20 v / v%, and other conditions are the same as those in embodiment 1.

[0098] Example 5

[0099] The difference between this embodiment and embodiment 1 is that when preparing the desulfurization and denitrification catalyst, the mass ratio of thiourea to activated carbon is 0.5:1, and other conditions are the same as those in embodiment 1.

[0100] Example 6

[0101] The difference between this embodiment and embodiment 1 is that when preparing the desulfurization and denitrification catalyst, the mass ratio of copper nitrate trihydrate, trimesic acid, and nitrogen-sulfur co-doped carbon material is 2.1:1:2.5, and other conditions are the same as those in embodiment 1.

[0102] Example 7

[0103] The difference between this embodiment and embodiment 1 is that the temperature during the deep treatment is 40° C., and the other conditions are the same as those in embodiment 1.

[0104] In order to better verify the effect of the present invention, a number of comparative examples are given below for detailed description.

[0105] Comparative Example 1

[0106] The difference between this comparative example and Example 1 is that the electric arc furnace dust is not calcined but directly made into slurry, and other conditions are the same as those in Example 1.

[0107] Comparative Example 2

[0108] The difference between this comparative example and Example 1 is that when preparing the calcined arc furnace dust slurry, the heating rate during the calcination of the arc furnace dust is 15°C / min, and the other conditions are the same as those in Example 1.

[0109] Comparative Example 3

[0110] The difference between this comparative example and Example 1 is that when preparing the calcined arc furnace dust slurry, the temperature of calcining the arc furnace dust is 950° C., and the other conditions are the same as those in Example 1.

[0111] Comparative Example 4

[0112] The difference between this comparative example and Example 1 is that the temperature during the pretreatment is 80° C., and the other conditions are the same as those in Example 1.

[0113] Comparative Example 5

[0114] The difference between this comparative example and Example 1 is that during the deep treatment, activated carbon is directly used without nitrogen and sulfur doping or copper modification, and other conditions are the same as those in Example 1.

[0115] Comparative Example 6

[0116] The difference between this comparative example and Example 1 is that when preparing the desulfurization and denitrification catalyst, the activated carbon is directly calcined in a nitrogen atmosphere without adding thiourea and without copper modification. Other conditions are the same as in Example 1.

[0117] Comparative Example 7

[0118] The difference between this comparative example and Example 1 is that when preparing the desulfurization and denitrification catalyst, the activated carbon is directly calcined in a nitrogen atmosphere without adding thiourea, and the other conditions are the same as those in Example 1.

[0119] Comparative Example 8

[0120] The difference between this comparative example and Example 1 is that when preparing the desulfurization and denitrification catalyst, the mass ratio of thiourea to activated carbon is 2:1, and the other conditions are the same as those in Example 1.

[0121] Comparative Example 9

[0122] The difference between this comparative example and Example 1 is that when preparing the desulfurization and denitration catalyst, copper is not used for modification, and the prepared nitrogen-sulfur co-doped carbon is directly used to load phosphomolybdic acid, and other conditions are the same as in Example 1.

[0123] Comparative Example 10

[0124] The difference between this comparative example and Example 1 is that when preparing the desulfurization and denitrification catalyst, the mass ratio of copper nitrate trihydrate, trimesic acid, and nitrogen-sulfur co-doped carbon material is 2.1:1:1, and other conditions are the same as those in Example 1.

[0125] Comparative Example 11

[0126] The difference between this comparative example and Example 1 is that when preparing the desulfurization and denitration catalyst, the calcination temperature of the copper-modified nitrogen-sulfur co-doped carbon material is 800° C., and the other conditions are the same as those in Example 1.

[0127] Comparative Example 12

[0128] The difference between this comparative example and Example 1 is that during the deep treatment, the treatment temperature is 80° C., and the other conditions are the same as those in Example 1.

[0129] The performance of the calcined arc furnace dust obtained in Examples 1-2 and Comparative Examples 2-3, the performance of the uncalcined arc furnace dust in Comparative Example 1, and the performance of the desulfurization and denitrification catalysts in Comparative Examples 5-11 were tested.

[0130] The test method is as follows:

[0131] The specific surface area and pore size distribution of the samples were determined using the ASAP 2020 fully automatic specific surface area and porosity analyzer produced by Micromeritics in the United States. The samples were first degassed at 300°C for 5 hours, and then the adsorption-desorption curve of N2 was determined by static physical adsorption method at liquid nitrogen temperature (-196°C). The specific surface area of ​​the samples was then calculated using the multi-point BET equation, and the pore size and total pore volume were calculated from the desorption curve of the samples using the Barrett-Joyner-Halenda (BJH) method.

[0132] The performance parameters of the calcined arc furnace dust of Examples 1-2 and Comparative Examples 1-3 are shown in Table 1, and the performance parameters of the desulfurization and denitrification catalysts of Examples 1, 5-6 and Comparative Examples 5-11 are shown in Table 2.

[0133] Table 1

[0134] <![CDATA[Specific surface area, m 2 / g]]> <![CDATA[Total pore volume, cm 3 / g]]> Average pore size, nm Example 1 3.55 0.015 13.29 Example 2 3.65 0.016 13.95 Comparative Example 1 4.65 0.018 14.12 Comparative Example 2 2.95 0.008 12.33 Comparative Example 3 2.81 0.006 12.12

[0135] From the test results in Table 1 above, it can be seen that under certain calcination conditions, the specific surface area, pore volume and average pore size of the calcined arc furnace dust are slightly reduced, mainly because after calcination, the crystallinity of zinc oxide and zinc ferrite in the arc furnace dust is enhanced, which is conducive to the improvement of desulfurization efficiency. However, if the heating rate is too high and the calcination temperature is too high during calcination, the specific surface area of ​​the material will be seriously affected, which is not conducive to the contact reaction between the gas and the calcined arc furnace dust. Therefore, it is necessary to reasonably control the calcination conditions of the arc furnace dust.

[0136] Table 2

[0137]

[0138]

[0139] It can be seen from the test results in Table 2 above that when preparing the desulfurization and denitration catalyst, the desulfurization and denitration catalyst prepared by the present invention has a suitable specific surface area, pore volume and average pore size by optimizing the preparation conditions. In Comparative Examples 5-8, the specific surface area of ​​the undoped activated carbon is higher, and the specific surface area, pore volume and pore size of the catalyst without adding thiourea are higher than those in Example 1. A large increase in thiourea will cause excessive doping of sulfur and nitrogen, and the specific surface area, pore volume and pore size of the catalyst will decrease significantly. The specific surface area, pore volume and pore size of the catalyst in Comparative Examples 9-11 are also lower than those in Example 1, mainly because the increase in the amount of copper modification and the excessively high calcination temperature will cause the agglomeration of copper particles on the surface of the nitrogen-sulfur doped carbon material.

[0140] The desulfurization and denitrification effects of the methods provided in the above embodiments and comparative examples are tested below. The test method and test results are as follows.

[0141] Test method: Use flue gas analyzer to detect the contents of sulfur dioxide, nitrogen monoxide, nitrogen dioxide and nitrous oxide at the gas inlet of the pretreatment tower and the gas outlet of the deep treatment tower respectively, and calculate the desulfurization and denitrification efficiency by the concentration changes of the above gases.

[0142] Desulfurization efficiency (%) = [(V1×N SO2 -V2×n SO2 ) / V1×N SO2 ]×100%.

[0143] Denitrification efficiency (%) = [(V1×N NO+NO2+N2O -V2×n NO+NO2+N2O ) / V1×N NO+NO2+N2O ]×100%.

[0144] Wherein, V1: the total volume of gas entering the pretreatment tower for treatment;

[0145] V2: total volume of gas discharged from the deep treatment tower;

[0146] N SO2 : The concentration of SO2 at the gas inlet of the pretreatment tower;

[0147] n SO2 : Total concentration of SO2 in the exhaust gas from the deep treatment tower

[0148] N NO+NO2+N2O: Total concentration of NO, NO2, and N2O at the gas inlet of the pretreatment tower;

[0149] n NO+NO2+N2O : The total concentration of NO, NO2 and N2O in the exhaust gas from the deep treatment tower.

[0150] The test results are shown in Table 3.

[0151] Table 3

[0152] Desulfurization efficiency, % Denitrification efficiency, % Example 1 99.8 98.5 Example 2 99.6 98.4 Example 3 99.7 98.5 Example 4 99.8 98.6 Example 5 99.3 98.2 Example 6 99.7 98.4 Example 7 99.5 98.2 Comparative Example 1 98.9 97.9 Comparative Example 2 99.2 98.0 Comparative Example 3 99.0 97.9 Comparative Example 4 97.8 96.5 Comparative Example 5 89.5 76.2 Comparative Example 6 93.1 85.5 Comparative Example 7 96.8 95.5 Comparative Example 8 98.5 97.1 Comparative Example 9 95.2 93.5 Comparative Example 10 98.3 97.0 Comparative Example 11 98.9 97.5 Comparative Example 12 99.1 98.1

[0153] It can be seen from the above test results that, compared with the comparative example, the present invention adopts calcined arc furnace dust slurry to pretreat the carbon black production tail gas, and then adopts copper-modified nitrogen-sulfur doped carbon material for deep treatment, and effectively optimizes the process conditions. The desulfurization efficiency is more than 99%, and the denitrification efficiency also reaches more than 98%.

[0154] It can also be seen from the above results that in Comparative Example 1, although the specific surface area and pore size of the uncalcined arc furnace dust are higher than those of the calcined arc furnace dust, the crystallinity of zinc oxide and zinc ferrite in the calcined arc furnace dust is improved, so the calcined arc furnace dust slurry is more effective in treating carbon black production exhaust gas.

[0155] The main reasons for the reduced desulfurization and denitrification efficiency in Comparative Examples 2 and 3 are: the heating rate during calcination is too fast, which is not conducive to the improvement of the crystallinity of zinc oxide and zinc ferrite; and the calcination temperature is too high, which will seriously reduce the specific surface area of ​​the calcined arc furnace dust, which is not conducive to the contact reaction between the calcined arc furnace dust and the gas.

[0156] It can be seen from the comparison between Comparative Examples 5-8 and Example 1 that although nitrogen-sulfur co-doped carbon will slightly reduce the specific surface area of ​​the material, it improves the desulfurization and denitrification efficiency of the material, mainly because the surface of the unmodified activated carbon is relatively smooth, and nitrogen-sulfur co-doping will destroy the original structure of the activated carbon, thereby making the catalyst surface rough and porous, which is more conducive to the adsorption of gas on the catalyst surface. Moreover, compared with the doping of a single element, the effect of nitrogen-sulfur co-doping is better, because the presence of N / S functional groups will produce more acid centers, active centers and oxygen vacancies on the catalyst surface, reduce the reaction energy barrier, and promote the adsorption and conversion of gases. However, if too much nitrogen and sulfur are doped, their penetration will destroy the original pores of the activated carbon, causing pore blockage, greatly reducing the specific surface area of ​​the catalyst.

[0157] It can be seen from the comparison between Comparative Examples 9-11 and Example 1 that a certain amount of copper modification can improve the catalytic activity of the catalyst. This is because copper modification can effectively improve the oxygen activation ability and active sites on the catalyst surface. However, excessive copper modification and excessive calcination temperature during the modification process will cause copper particles to agglomerate on the catalyst surface, thereby reducing the specific surface area and active sites of the catalyst.

[0158] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A highly efficient method for treating waste gas, characterized in that: The following steps are involved: S1: calcining the electric arc furnace dust in an oxygen atmosphere at 750-850° C. for 1-2 hours, adding the calcined electric arc furnace dust into water and stirring to prepare a calcined electric arc furnace dust slurry with a solid content of 5-10wt%; S2: The tail gas from carbon black production is sequentially fed into a pretreatment tower and treated with calcined arc furnace dust slurry; S3: the tail gas enters a deep treatment tower and is deeply treated under the catalysis of a desulfurization and denitration catalyst, wherein the desulfurization and denitration catalyst is obtained by using a copper-modified nitrogen-sulfur co-doped carbon material as a carrier and loaded with phosphomolybdic acid; S4: The tail gas after deep treatment enters the absorption tower for absorption treatment.

2. The method for efficiently treating waste gas according to claim 1, characterized in that: In step S1, the heating rate during the calcination treatment is 8-10°C / min.

3. The efficient waste gas treatment method according to claim 1, characterized in that: In step S2, when a pretreatment tower is used for treatment, the step of introducing oxygen into the pretreatment tower is also included, during which the carbon black production tail gas is premixed with oxygen to obtain a mixed gas, and a preheating treatment is performed, and the preheating temperature is 50-60°C; and / or the oxygen content in the mixed gas is 10-20v / v%; and / or the temperature during pretreatment is 50-60°C; and / or during pretreatment, the amount ratio of the calcined arc furnace dust slurry to the mixed gas is (5-10)g:1Nm 3 The introduction rate of the mixed gas is 300-400ml / min.

4. The high-efficiency waste gas treatment method according to claim 1, characterized in that: In step S3, the method for preparing the desulfurization and denitration catalyst comprises the following steps:

1. Using activated carbon as a matrix and thiourea as a doping raw material, calcining is performed in a nitrogen atmosphere to obtain a nitrogen-sulfur co-doped carbon material; the nitrogen-sulfur co-doped carbon material is dispersed in a solvent, and then a copper source and trimesic acid are added, mixed evenly, and then placed in a reactor for reaction, and the solid obtained by the reaction is dried and calcined to obtain a copper-modified nitrogen-sulfur co-doped carbon material; 2. After dispersing the copper-modified nitrogen-sulfur co-doped carbon material, add hydrochloric acid solution to adjust the pH, then add phosphomolybdic acid dispersion, perform ultrasonic treatment, and then dry to obtain a desulfurization and denitrification catalyst.

5. The high-efficiency waste gas treatment method according to claim 4, characterized in that: In step one, when preparing nitrogen-sulfur co-doped carbon material, the mass ratio of thiourea to activated carbon is (0.5-1.5):1; and / or the temperature during calcination treatment is 490-510°C; and / or the heating rate during calcination treatment is 5-10°C / min; and / or the calcination treatment time is 1-2h; and / or the nitrogen flow rate during calcination treatment is 100-120ml / min.

6. The high-efficiency waste gas treatment method according to claim 4, characterized in that: In step 1, the copper source is copper nitrate trihydrate; and / or the mass ratio of the copper source, trimesic acid, and nitrogen-sulfur co-doped carbon material is 2.1:(1-2):(2-2.5); and / or the solvent is a mixture of DMF, water and ethanol, and the volume ratio of DMF, water and ethanol is 1:1:1; and / or the reaction temperature is 80-90°C and the reaction time is 20-30h.

7. The high-efficiency waste gas treatment method according to claim 4, characterized in that: In step one, when preparing copper-modified nitrogen-sulfur co-doped carbon material, the atmosphere during calcination is a nitrogen atmosphere, and the nitrogen flow rate during calcination is 100-120 ml / min; and / or the calcination temperature is 550-600°C, the calcination time is 1-2h; and / or the heating rate during calcination is 5-10°C / min.

8. The high-efficiency waste gas treatment method according to claim 4, characterized in that: In step 2, the concentration of the hydrochloric acid solution is 1-1.5 mol / L, and the pH is adjusted to 3-3.5; and / or the concentration of the phosphomolybdic acid dispersion is 0.05-0.1 g / ml; and / or the mass ratio of the copper-modified nitrogen-sulfur co-doped carbon material to the phosphomolybdic acid is 1:(0.1-0.5).

9. The high-efficiency waste gas treatment method according to claim 1, characterized in that: In step S3, the deep treatment further includes the step of mixing the tail gas discharged from the pretreatment tower with oxygen, wherein the concentration of oxygen in the mixed gas is 5-10 v / v%; and / or the weight hourly space velocity of the gas during the deep treatment is (4900-5000) ml·h -1 ·g -1 ; and / or the temperature during deep treatment is 40-60°C.

10. The high-efficiency waste gas treatment method according to claim 1, characterized in that: The following steps are also included: The exhaust gas after absorption treatment is tested by a flue gas analyzer to detect the concentration of nitrogen oxides and sulfur oxides in the exhaust gas. If the concentration of nitrogen oxides and sulfur oxides reaches the emission standard, they will be discharged directly, otherwise the exhaust gas will continue to be absorbed.