Acid anhydride modified Cu-coated NH2-UiO-66 (Zr) catalyst for preparing acetic acid through photo-reduction of CO2 as well as preparation method and application of acid anhydride modified Cu-coated NH2-UiO-66 (Zr) catalyst

The Cu@NH2-UiO-66(Zr) photocatalyst is modified by acid anhydride to form a hydrophobic and gas-solid-liquid three-phase microenvironment, which solves the problem of low CO2 reduction activity and selectivity in the existing technology and achieves efficient CO2 Converted to acetic acid with excellent stability and low cost.

CN118847221APending Publication Date: 2024-10-29SICHUAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410859919.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing photocatalysts have low CO2 reduction activity and selectivity in aqueous solution, and the yield and selectivity of C2 products such as acetic acid are low, making it difficult to achieve efficient CO2 conversion.

Method used

Anhydride-modified Cu@NH2-UiO-66(Zr) photocatalyst is used to improve the hydrophobicity of the catalyst through the acid anhydride modification step in the preparation process, forming a gas-solid-liquid three-phase microenvironment to enhance the concentration and active sites of CO2 , promote CO2 reduction reaction.

Benefits of technology

Efficient photocatalytic reduction of CO2 to acetic acid was achieved, with a yield as high as 188.7 μmol g-1h-1, a selectivity close to 100%, and excellent photocatalytic stability and low cost, making it suitable for long-term reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847221A_ABST
    Figure CN118847221A_ABST
Patent Text Reader

Abstract

The invention discloses an acid anhydride modified Cu (at) NH2-UiO-66 (Zr) catalyst for photoreduction of CO2 to prepare acetic acid as well as a preparation method and application of the acid anhydride modified Cu (at) NH2-UiO-66 (Zr) catalyst. The preparation method comprises the following steps: dissolving ZrCl4 and 2-aminoterephthalic acid in N, N-dimethylformamide, and carrying out a reaction so as to obtain NH2-UiO-66 (Zr); the preparation method comprises the following steps: activating NH2-UiO-66 (Zr), carrying out ultrasonic dispersion, dropwise adding a Cu (NO3) 2.3 H2O aqueous solution, and reacting to obtain Cu (at) NH2-UiO-66 (Zr); the preparation method comprises the following steps: reacting Cu (at) NH2-UiO-66 (Zr) with acid anhydride to obtain Cu (at) NH2-UiO-66 (Zr)-C; the anhydride modified Cu (at) NH2-UiO-66 (Zr) photocatalyst prepared by the preparation method disclosed by the invention can be used for efficiently photo-reducing CO2 into acetic acid, and the yield is up to 188.7 mu mol g <-1 > h <-1 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalysis, and in particular to an anhydride-modified Cu@NH2-UiO-66(Zr) photoreduction catalyst for producing acetic acid by CO2, and a preparation method and application thereof. Background Art

[0002] In addition to being the main component of greenhouse gases, CO2 is also a safe, cheap and abundant carbon source that can be converted into other useful chemical fuels. Converting CO2 into valuable organic matter such as C1 and C2 can not only alleviate the greenhouse effect, but also provide important chemical raw materials for human production and alleviate the energy crisis. Therefore, the development of effective technologies to achieve CO2 fixation and conversion has received great attention from researchers.

[0003] After years of development, researchers have developed different CO2 conversion technologies, including chemical conversion, biological conversion, thermal catalysis, electrocatalysis, and photocatalysis. It is worth pointing out that CO2 is a thermodynamically very stable compound. When it is converted and utilized, CO2 must be activated, that is, a high amount of energy must be input into CO2. In other words, any large-scale use of CO2 process has potential energy consumption. Therefore, the development of low-energy CO2 conversion and utilization technology is of great significance to the establishment of a decarbonized energy system.

[0004] Artificial photosynthesis is an innovative technology for the conversion and utilization of CO2. Photocatalytic CO2 reduction uses clean, renewable and abundant solar energy to excite semiconductor photocatalytic materials to produce photogenerated electrons and holes to convert CO2 into high-value hydrocarbons. Compared with other methods, this process is carried out at room temperature and pressure, with mild operating conditions, simple and easy-to-obtain raw materials, and direct use of solar energy without the need for auxiliary energy. It can truly achieve the recycling of carbon materials and is therefore considered to be a highly potential technical means to reduce the concentration of CO2 in the atmosphere and alleviate the energy crisis. The preparation of efficient and highly selective photocatalysts that can be used for photocatalytic CO2 reduction is the focus of research on photocatalytic CO2 reduction.

[0005] Among the many catalysts, metal organic framework photocatalysts are ideal materials for designing photocatalytic CO2 reduction catalysts due to their high specific surface area, high porosity, abundant metal oxygen sites and structural adjustability. However, most of the CO2 reduction systems reported so far need to be carried out in organic solvents and alcohols or amines as sacrificial agents. In comparison, using aqueous solution as a reaction medium for CO2 reduction is more economical and environmentally friendly. However, the saturated solubility of CO2 in water is very low (about 33mM at room temperature and pressure), and the diffusion coefficient in the liquid phase is extremely limited (about 1×10 - 5 cm 2s -1 ), which greatly reduces the activity and selectivity of CO2 reduction. Previous studies have found that after bubbling CO2 into the aqueous phase, the photocatalytic activity of the nanoparticle dispersion system is much better than that of the non-bubbling system, indicating that the construction of a gas-solid-liquid three-phase microenvironment can effectively promote the CO2 reduction process. However, there are still few studies in this area, and the only reports are mainly focused on semiconductors and metal materials. There are few reports on three-phase photocatalytic CO2 reduction based on hydrophobic MOFs. In addition, in current photocatalyst research, due to the difficulty of CC coupling, the products are mainly C1, and there are fewer C2 products with higher value; in existing research on the production of acetic acid (CH3COOH), the yield and selectivity of CH3COOH are low. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide an anhydride-modified Cu@NH2-UiO-66(Zr) photoreduction catalyst for CO2 to produce acetic acid, and a preparation method and application thereof.

[0007] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:

[0008] In the first aspect, a method for preparing an anhydride-modified Cu@NH2-UiO-66(Zr) photoreduction catalyst for producing acetic acid by CO2 (hereinafter referred to as anhydride-modified Cu@NH2-UiO-66(Zr) photocatalyst) is provided, which comprises the following steps:

[0009] Step 1, dissolving ZrCl4 and 2-aminoterephthalic acid in N,N-dimethylformamide, heating for reaction, filtering, washing, and drying to obtain NH2-UiO-66(Zr) after the reaction is completed;

[0010] Step 2, activating NH2-UiO-66(Zr), ultrasonically dispersing, adding Cu(NO3)2·3H2O aqueous solution dropwise and stirring vigorously, then adding NaBH4 solution, after the reaction is completed, filtering the obtained solution, washing, and vacuum drying to obtain Cu@NH2-UiO-66(Zr);

[0011] Step 3: react Cu@NH2-UiO-66(Zr) with acid anhydride. After the reaction is completed, filter, wash and dry to obtain Cu@NH2-UiO-66(Zr)-C.

[0012] Furthermore, in step 1, the heating conditions are: heating at 120° C. for 24 hours.

[0013] Furthermore, in step 2, the activation conditions are: activation at 150° C. for 12 h; and the ultrasonic dispersion conditions are: adding anhydrous n-hexane and ultrasonicating for 1 h.

[0014] Furthermore, after the ultrasonic dispersion was completed, a 0.5% wt Cu(NO3)2·3H2O aqueous solution was added dropwise and stirred vigorously for 2 h. After the stirring was completed, a NaBH4 solution was added and the stirring was continued for 2 h.

[0015] Furthermore, in step 3, the reaction conditions are: reacting in an oil bath at 80° C. for 24 hours.

[0016] In the second aspect, the application of anhydride-modified Cu@NH2-UiO-66(Zr) photocatalyst in photocatalytic CO2 reduction is provided.

[0017] The beneficial effects of the present invention are:

[0018] (1) The anhydride-modified Cu@NH2-UiO-66(Zr) photocatalyst prepared by the present invention can efficiently photoreduced CO2 to CH3COOH with a yield of up to 188.7 μmol g -1 h -1 .

[0019] (2) The photocatalyst prepared by the present invention has high activity and high selectivity, which exceeds most of the CH3COOH-producing photocatalysts reported so far, and the CH3COOH selectivity is close to 100%.

[0020] (3) The hydrophobic Cu@NH2-UiO-66(Zr)-C photocatalyst provided by the present invention has excellent photocatalytic stability and is suitable for long-term photocatalytic CO2 reduction reaction.

[0021] (4) The hydrophobic Cu@NH2-UiO-66(Zr)-C catalyst provided by the present invention does not use precious metals and rare earth metals in the preparation process, and only uses conventional chemical reagents, which has lower cost and better effect, and has excellent market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is the X-ray diffraction pattern of the anhydride-modified Cu@NH2-UiO-66(Zr) photocatalyst obtained in Example 5;

[0023] Figure 2 is the Fourier transform infrared spectrum of the anhydride modified Cu@NH2-UiO-66(Zr) photocatalyst obtained in Example 5;

[0024] Figure 3 This is the NMR structure of the anhydride-modified Cu@NH2-UiO-66(Zr) photocatalyst obtained in Example 5;

[0025] Figure 4This is a transmission electron microscopy image of the anhydride-modified Cu@NH2-UiO-66(Zr) photocatalyst obtained in Example 5;

[0026] Figure 5 The contact angle diagram of the anhydride-modified Cu@NH2-UiO-66(Zr) photocatalyst obtained in Example 5;

[0027] Figure 6 The photocatalysts obtained in Comparative Example 1 and Examples 1 to 4 are dispersed in water;

[0028] Figure 7 The photos are of the catalysts obtained in Comparative Example 1, Example 1 and Example 5 dispersed in water;

[0029] Figure 8 The photocatalytic performance curves of the photocatalysts prepared in Examples 1 to 4 and Comparative Example 1 under visible light irradiation of 800nm>λ>400nm;

[0030] Fig. 9 The photocatalytic performance curves of the photocatalysts prepared in Examples 1, 5 and Comparative Example 1 under visible light irradiation of 800nm>λ>400nm;

[0031] Fig.10 The photoelectric properties of the photocatalysts prepared in Example 5 and Comparative Example 1; wherein a is the photocurrent response curve of Cu@NH2-UiO-66(Zr)-anhydride and Cu@NH2-UiO-66(Zr) catalysts under simulated intermittent illumination; b is electrochemical impedance spectroscopy (EIS); c is photoluminescence (PL) test;

[0032] Fig.11 This is a performance stability test of the photocatalyst prepared in Example 5. DETAILED DESCRIPTION

[0033] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0034] The material performance was evaluated using a photocatalytic CO2 reduction evaluation system. The light source for the photocatalytic experiment was a 300W xenon lamp with a 400nm cutoff filter and an infrared cutoff filter as a visible light source. The light intensity of the catalytic reaction (λ = 400-800nm) was 56mW / cm 2 (Note: The distance between the light source and the reactor is 11 cm).

[0035] In the following examples, the reagents used are: analytical grade zirconium chloride (ZrCl4), 2-aminoterephthalic acid (H2ATA), N,N-dimethylformamide (DMF) purchased from Sigma Aldrich, methanol (CH3OH), anhydrous n-hexane, copper nitrate trihydrate (Cu(NO3)2·3H2O), sodium borohydride (NaBH4), ethanol (CH3CH2OH), hexanoic anhydride, acetonitrile (CH3CN) purchased from Shanghai MacLean Reagent Co., Ltd.

[0036] All the above chemicals were used directly without further purification.

[0037] Example 1

[0038] Example 1 is a 2 mmol hexanoic anhydride modified Cu@NH2-UiO-66(Zr) photocatalyst, and its preparation method comprises the following steps:

[0039] Preparation of NH2-UiO-66(Zr):

[0040] (1) Weigh 0.240 g of ZrCl4 and 0.1860 g of 2-aminoterephthalic acid and dissolve them in 60 ml of N,N-dimethylformamide and 0.19 ml of deionized water.

[0041] (2) The solution obtained in (1) was transferred to a 100 ml reaction kettle and heated at 120°C for 24 h.

[0042] (3) After the reaction is completed, filter, wash, and then dry to obtain white NH2-UiO-66(Zr) powder.

[0043] Preparation of Cu@NH2-UiO-66(Zr):

[0044] (4) Weigh 100 mg of the NH2-UiO-66(Zr) powder obtained in (3) and activate it at 150°C for 12 h.

[0045] (5) After activation, add 20 ml of anhydrous n-hexane and sonicate for 1 h.

[0046] (6) After ultrasonic dispersion, 12.5 uL of 0.5% wt Cu(NO3)2·3H2O aqueous solution was added dropwise and stirred vigorously for 2 h.

[0047] (7) After stirring, add NaBH4 solution and continue stirring for 2 h.

[0048] (8) After the reaction is completed, the resulting solution is filtered, washed, and vacuum dried to obtain the product Cu@NH2-UiO-66(Zr).

[0049] Preparation of Cu@NH2-UiO-66(Zr)-C:

[0050] (9) 87.7 mg of Cu@NH2-UiO-66(Zr) obtained in (8) and 2 mmol of n-hexanoic anhydride were dissolved in 5 ml of acetonitrile and then reacted in an oil bath at 80°C for 24 h.

[0051] (10) After the reaction was completed, the mixture was filtered, washed with CHCl3 several times, and dried in vacuo to obtain the final sample Cu@NH2-UiO-66(Zr)-C6-2.

[0052] The prepared samples were subjected to photocatalytic CO2 reduction.

[0053] The test method is as follows: 20 mg of the photocatalyst Cu@NH2-UiO-66(Zr)-C6-2 is ultrasonically dispersed in 20 ml of deionized water and 40 ul of triethanolamine (TEOA). After the temperature reaches 6°C through a circulating water cooling system, the mixture is placed in a reactor and irradiated with light for 6 hours. The gas phase product is detected by an online reaction system equipped with a gas chromatograph, and the liquid phase product is detected by an online reaction system equipped with a gas chromatograph. 1 H NMR analysis was performed by adding 0.5 mL of the liquid product into 0.1 mL of D2O, with 5 μL of phenol as the internal standard.

[0054] Example 2

[0055] In the method steps of Example 2, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. In Example 2, n-hexanoic anhydride is replaced with butyric anhydride, and the remaining steps are consistent with those of Example 1, to obtain Cu@NH2-UiO-66(Zr)-C4-2.

[0056] Example 3

[0057] In the method steps of Example 3, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. In Example 3, n-hexanoic anhydride is replaced with valeric anhydride, and the remaining steps are consistent with those of Example 1 to prepare Cu@NH2-UiO-66(Zr)-C5-2.

[0058] Example 4

[0059] In the method steps of Example 4, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. In Example 4, n-hexanoic anhydride is replaced with decanoic anhydride, and the remaining steps are consistent with those of Example 1 to prepare Cu@NH2-UiO-66(Zr)-C10-2.

[0060] Example 5

[0061] In the method steps of Example 5, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. This example is to control the amount of n-hexanoic anhydride. The content of n-hexanoic anhydride in Example 1 is changed to 0.15 mmol, and the remaining steps are consistent with Example 1.

[0062] Comparative Example 1

[0063] In the method steps of Comparative Example 1, the same points as those of Example 1 are not described here, and only the differences from Example 1 are described. This comparative example prepares Cu@NH2-UiO-66(Zr) without acid anhydride modification.

[0064] Reference Figure 1 , the X-ray diffraction pattern of Cu@NH2-UiO-66(Zr)-anhydride is similar to that of Cu@NH2-UiO-66(Zr), indicating that the anhydride treatment did not significantly change the crystal structure of the Cu@NH2-UiO-66(Zr) catalyst.

[0065] Reference Figure 2 According to the Fourier transform infrared spectrum, after anhydride modification, the -1 Typical hydrocarbon stretching vibration signals can be observed at 1685 cm -1 The vibration signal of amide after the reaction of -NH2 and acid anhydride also appeared, indicating that the acid anhydride successfully modified Cu@NH2-UiO-66(Zr).

[0066] Reference Figure 3 From the H-NMR spectrum, we can see that after the anhydride modification, the chemical shift of H corresponding to the anhydride monomer appears, indicating the successful modification of the anhydride on Cu@NH2-UiO-66(Zr); in addition, the content of the anhydride was quantified by the H-NMR spectrum, where the theoretical feed ratio of the anhydride accounted for 50% of the -NH2 content in Cu@NH2-UiO-66(Zr), and the actual content after the reaction was 31%.

[0067] Reference Figure 4 The surface morphology of Cu@NH2-UiO-66(Zr)-anhydride was characterized by transmission electron microscopy and high-angle annular dark field scanning transmission electron microscopy. Cu@NH2-UiO-66(Zr)-anhydride is still in the shape of a regular octahedron, and its surface nanostructure is not significantly different from that of Cu@NH2-UiO-66(Zr), indicating that the morphology remains intact after anhydride modification. In addition, there is no obvious deposition of metal nanoparticles on the surface of MOF, and the uniform distribution of Cu elements can be seen from the EDS image, indicating that the Cu nanoparticles are inside the pores of MOF.

[0068] Reference Figure 5The wettability of the catalyst before and after anhydride modification was investigated by contact angle. The untreated Cu@NH2-UiO-66(Zr) was hydrophilic with a contact angle of 26°; the contact angle of Cu@NH2-UiO-66(Zr)-anhydride was 134°, which was hydrophobic.

[0069] Reference Figure 6-7 , the dispersion of the sample in aqueous solution further proved the hydrophilic and hydrophobic properties of the sample, indicating that anhydride treatment is an effective method to improve the hydrophobicity of Cu@NH2-UiO-66(Zr).

[0070] The contact angle of the Cu@NH2-UiO-66(Zr) catalyst without anhydride modification is less than 90°, and it can be dispersed in water very evenly, indicating that Cu@NH2-UiO-66(Zr) is hydrophilic. In contrast, the catalysts prepared in Examples 1, 3, and 4 have a contact angle of about 120° and cannot be dispersed in water, indicating that the catalyst is hydrophobic, proving the successful modification of the catalyst.

[0071] The photocatalysts prepared in Examples 1 to 4 and Comparative Example 1 were subjected to a performance comparison test. Figure 8It can be seen from the performance test diagram that the acetic acid production rate is Cu@NH2-UiO-66(Zr)-C6-2>Cu@NH2-UiO-66(Zr)-C5-2>Cu@NH2-UiO-66(Zr)-C10-2>Cu@NH2-UiO-66(Zr)-C4-2≈Cu@NH2-UiO-66(Zr). The contact angle results of the Cu@NH2-UiO-66(Zr)-C4-2 catalyst prepared in Example 2 show that it is hydrophilic, and its acetic acid yield is similar to that of the Cu@NH2-UiO-66(Zr) catalyst prepared in Comparative Example 1. The photocatalytic CO2 reduction and acetic acid production rates of the Cu@NH2-UiO-66(Zr)-C6, Cu@NH2-UiO-66(Zr)-C5 and Cu@NH2-UiO-66(Zr)-C10 catalysts prepared in Examples 1, 3 and 4 are all higher than those of Cu@NH2-UiO-66(Zr), indicating that the hydrophobic catalyst obtained by anhydride-modified Cu@NH2-UiO-66(Zr) is beneficial to the improvement of the photocatalytic CO2 reduction performance. While the Cu@NH2-UiO-66(Zr)-C6, Cu@NH2-UiO-66(Zr)-C5 and Cu@NH2-UiO-66(Zr)-C10 catalysts have similar hydrophobicity, they have different photoreduction performances for CO2. This indicates that in addition to the hydrophobicity of the photocatalyst, the photocatalytic performance of the catalyst may also be affected by the steric effect of the alkyl anhydride. The actual anhydride contents of the three catalysts are Cu@NH2-UiO-66(Zr)-C5>Cu@NH2-UiO-66(Zr)-C6>Cu@NH2-UiO-66(Zr)-C10. The actual anhydride content of Cu@NH2-UiO-66(Zr)-C5 is the highest, which may block the MOF pores. Although the actual anhydride content of Cu@NH2-UiO-66(Zr)-C10 is the lowest, the anhydride chain length is the longest, which may also block the pores of Cu@NH2-UiO-66(Zr), cover the active sites, and affect the mass transfer of CO2 and adsorption and reaction intermediates, thus leading to a decrease in activity. Therefore, the acetic acid yield of Cu@NH2-UiO-66(Zr)-C6 is higher than that of Cu@NH2-UiO-66(Zr)-C5 and Cu@NH2-UiO-66(Zr)-C10.

[0072] The photocatalysts prepared in Examples 1 and 5 and Comparative Example 1 were subjected to a performance comparison test. Fig. 9It can be seen from the performance test diagram that the acetic acid production rate is Cu@NH2-UiO-66(Zr)-C6-0.15>Cu@NH2-UiO-66(Zr)-C6-2>Cu@NH2-UiO-66(Zr). The 6h acetic acid yield of Cu@NH2-UiO-66(Zr)-C6-0.15 can reach 188.7μmol g -1 h -1 When the theoretical feed ratio of alkyl anhydride is greater than or equal to 0.15 mmol, the catalyst is hydrophobic, and the hydrophobicity of Cu@NH2-UiO-66(Zr)-C6-0.15 is similar to that of Cu@NH2-UiO-66(Zr)-C6-2. However, the acetic acid yield of Cu@NH2-UiO-66(Zr)-C6-0.15 is 188.7 μmol·g -1 ·h -1 , which is higher than that of Cu@NH2-UiO-66(Zr)-C6-2, indicating that steric hindrance is indeed another important factor affecting CO2 photoreduction.

[0073] Reference Fig.10 , Fig.10 a is the photocurrent response curve of Cu@NH2-UiO-66(Zr)-anhydride and Cu@NH2-UiO-66(Zr)-catalysts under simulated intermittent illumination. Under Ar and CO2 conditions, Cu@NH2-UiO-66(Zr)-anhydride showed a higher photocurrent response density than Cu@NH2-UiO-66(Zr), indicating that Cu@NH2-UiO-66(Zr)-anhydride is more conducive to the separation of photogenerated carriers and electrons are more easily captured by CO2. Fig.10 b is the electrochemical impedance spectroscopy (EIS) analysis, the semicircle radius of Cu@NH2-UiO-66(Zr)-anhydride is smaller than that of Cu@NH2-UiO-66(Zr), indicating that the charge transfer resistance of Cu@NH2-UiO-66(Zr)-anhydride is smaller; Fig.10 c is the photoluminescence (PL) test. The emission intensity of Cu@NH2-UiO-66(Zr)-anhydride is weaker than that of Cu@NH2-UiO-66(Zr), indicating that anhydride modification can further promote the migration and separation of photogenerated electron-hole pairs. The above results show that Cu@NH2-UiO-66(Zr)-anhydride can effectively inhibit the recombination of photogenerated carriers and significantly enhance the migration of electron-hole pairs, thereby further improving the photocatalytic activity.

[0074] Reference Fig.11 , the 24h acetic acid yield of Cu@NH2-UiO-66(Zr)-C6-0.15 remained basically unchanged.

[0075] In summary, the present invention uses acid anhydride to modify the amino group of Cu@NH2-UiO-66(Zr) to improve the hydrophobicity of the catalyst, form a gas-solid-liquid three-phase reaction interface on the catalyst surface, increase the concentration of CO2 in the active sites on the catalyst surface, and thus improve the reduction activity and selectivity of CO2.

[0076] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing anhydride-modified Cu@NH2-UiO-66(Zr) catalyst for photoreduction of CO2 to acetic acid, characterized in that: The following steps are involved: Step 1, dissolving ZrCl4 and 2-aminoterephthalic acid in N,N-dimethylformamide, heating for reaction, filtering, washing, and drying to obtain NH2-UiO-66(Zr) after the reaction is completed; Step 2, activating NH2-UiO-66(Zr), ultrasonically dispersing, adding Cu(NO3)2·3H2O aqueous solution dropwise and stirring vigorously, then adding NaBH4 solution, after the reaction is completed, filtering the obtained solution, washing, and vacuum drying to obtain Cu@NH2-UiO-66(Zr); Step 3: react Cu@NH2-UiO-66(Zr) with acid anhydride. After the reaction is completed, filter, wash and dry to obtain Cu@NH2-UiO-66(Zr)-C.

2. The method for preparing the anhydride-modified Cu@NH2-UiO-66(Zr) photoreduction catalyst for producing acetic acid by CO2 according to claim 1, characterized in that: In step 1, the heating condition is: heating at 120° C. for 24 h.

3. The method for preparing the anhydride-modified Cu@NH2-UiO-66(Zr) photoreduction catalyst for producing acetic acid by CO2 according to claim 1, characterized in that: In step 2, the activation conditions are: activation at 150° C. for 12 h; and the ultrasonic dispersion conditions are: adding anhydrous n-hexane and ultrasonicating for 1 h.

4. The method for preparing the anhydride-modified Cu@NH2-UiO-66(Zr) photoreduction catalyst for producing acetic acid by CO2 according to claim 3, characterized in that: After ultrasonic dispersion was completed, 0.5% wt Cu(NO3)2·3H2O aqueous solution was added dropwise and stirred vigorously for 2 h. After stirring was completed, NaBH4 solution was added and stirring was continued for 2 h.

5. The method for preparing the anhydride-modified Cu@NH2-UiO-66(Zr) photoreduction catalyst for producing acetic acid by CO2 according to claim 1, characterized in that: In step 3, the reaction conditions are: reacting in an oil bath at 80° C. for 24 h.

6. Anhydride-modified Cu@NH2-UiO-66(Zr) catalyst for photoreduction of CO2 to acetic acid prepared by the method described in any one of claims 1 to 5.

7. Use of the anhydride-modified Cu@NH2-UiO-66(Zr) photoreduction of CO2 to acetic acid catalyst according to claim 6 in photocatalytic CO2 reduction to acetic acid.

Citation Information

Patent Citations

  • Hollow UiO-66-NH2 (MZr) encapsulated metal particle and preparation method and application thereof

    CN115007210A

  • Modified uio-66-NH2 material, its preparation procedure and the use thereof

    EP4309783A1