Subcritical zone ultra-fine grain rolling method for medium carbon steel bar

By carrying out the ultra-fine grain rolling method in the subcritical zone of medium carbon steel bars with accumulated ultra-large torsional deformation in the subcritical zone of ferrite and pearlite, the problems of poor permeability and high forming load in the existing technology are solved and achieved. The increase in grain refinement and reduction in energy consumption meet the needs of high-performance materials.

CN118847697AInactive Publication Date: 2024-10-29NANJING IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410963645.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing ultrafine-grained material preparation technology has problems such as poor permeability, high forming load, and insufficient grain refinement in large-size bulk materials, making it difficult to meet the needs of industrial-grade large-size full-body ultrafine-grained materials.

Method used

Using the ultra-fine grain rolling method in the subcritical zone of medium carbon steel bars that accumulates large torsional deformation in the subcritical zone of ferrite and pearlite, the deformation tool is designed through finite element simulation, and the shape and parameters of the roll and guide plate are adjusted to achieve The spiral movement and heating treatment of the blank during the rolling process ensure the torsion angle and area reduction rate in the deformation zone, and improve the degree of grain refinement.

Benefits of technology

It significantly expands the degree of grain refinement, improves material performance, and reduces energy consumption with relatively low-temperature processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847697A_ABST
    Figure CN118847697A_ABST
Patent Text Reader

Abstract

The invention discloses an ultra-fine grain rolling method for a medium carbon steel bar in a subcritical zone. The method belongs to the technical field of ultra-fine grain bar preparation and comprises the following operation steps that (1) a deformation tool is designed, and deformation parameters are determined; (2) machining, preparing and installing a deformation tool; step (3), deformation parameter adjustment; (4) heating the blank; and (5) a rolling test is conducted. According to the rolling method, through compression and torsion composite plastic deformation formed by spiral movement of the blank, full-body super-large plastic deformation with the accumulation area reduction rate reaching up to 73% is achieved, the grain refinement degree can be further improved, and therefore the requirement for higher use performance is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ultrafine grain bar preparation, and in particular relates to a subcritical zone ultrafine grain rolling method for a medium carbon steel bar. Background Art

[0002] In recent years, ultrafine grain / nanocrystalline materials have attracted the attention of experts in the field of materials around the world due to their excellent performance. People have continuously improved the strength and toughness of polycrystalline materials by continuously refining the grains. Among them, the research results of severe plastic deformation (Severe Plastic Deformation, referred to as SPD) technology are particularly eye-catching. At present, the mainstream SPD processes include high pressure torsion (HPT), equal channel angular extrusion (ECAP), cumulative rolling (ARB), multi-directional forging (MF) and torsional extrusion (TE). However, these SPD methods also have obvious limitations, mainly manifested in the following aspects: (1) The permeability of the violent deformation zone is poor, which only occurs near the workpiece-mold or workpiece-workpiece surface and does not penetrate into the core of the workpiece, that is, the penetration depth of the deformation zone is small or the penetration capacity is poor, which is far from meeting the requirements for the preparation of industrial-grade large-scale ultrafine-grained materials; (2) In the deformation process of the existing SPD technology, sufficiently large hydrostatic pressure plays an important role in suppressing deformation defects such as cracks and constraining the free deformation of materials to enhance the deformation accumulation effect. As a result, the forming load of various existing SPD methods (average unit pressure reaches GPa level) is much higher than that of conventional plastic deformation methods (generally MPa level), which seriously restricts the engineering application of SPD technology in the field of large-scale bulk material preparation.

[0003] There are relatively few reports on the ultrafine grain process of medium carbon steel at home and abroad. However, due to the advantages of ultrafine grain steel such as excellent fatigue resistance, good weldability, high strength and good low temperature toughness, its broad application prospects in the processing field are unquestionable.

[0004] A Chinese patent (publication number: CN 103572023 B) proposes a method for manufacturing ultra-fine grains on the surface of a low-alloy steel thick plate / extra-thick plate. The method uses multiple controlled rolling and controlled cooling to refine the surface austenite grains, and quickly cools to obtain a thick steel plate with a surface fine grain structure. Although an 80mm thick plate is produced, the refinement effect of the surface structure and the core structure is significantly different. The deformation does not penetrate into the core, and only the surface (1 to 10mm) range is fine grained.

[0005] Chinese patent (publication number: CN 110408869 A) proposes a method for preparing ultrafine grain copper and copper alloy wires and rods. The method first anneals the material to obtain an equiaxed crystal structure with a grain size range of 20 to 250 μm; then, the material is subjected to torsion and extrusion deformation to obtain a copper rod with a diameter of 10 mm and a length of 80 mm. The obtained copper rod is not only small in size, but also has a grain size that is obviously gradient distributed, with an edge grain size of about 2 μm and a core grain size of about 100 μm, which is difficult to meet market demand.

[0006] The Chinese patent (CN 109127754 A) mentions a method for preparing ultrafine-grained magnesium alloy extruded rods. The magnesium alloy is twisted while being extruded, so that it undergoes plastic deformation under the action of the composite stress field formed by tensile stress and torsional stress. This patent avoids the size of the finished product, and the torsion amount is small, the shear deformation is small, and the grains cannot be ultra-fine.

[0007] The Chinese patent (CN 103290296 A) mentions an ultrafine-grained large-size tungsten rod and its preparation method, which belongs to the field of powder metallurgy. The doped tungsten powder is obtained by reducing the doped blue tungsten powder at H2 and 600-800°C, and the doped tungsten powder is cold isostatically pressed and sintered to obtain an ultrafine-grained large-size tungsten alloy. Although the diameter of the finished rod exceeds 57mm, the degree of grain refinement is not significant (grain size>5μm), which cannot meet the requirements of high-performance and high-tech materials.

[0008] The forming principle is as follows: based on the oblique rolling forming principle, a single tapered roller is used and the blank enters from the large diameter end of the tapered roller to form a single tapered deformation zone. The deformation zone adopts an ultra-large feed angle (22°), rolling angle (23.5°) and an ultra-long deformation zone (the ratio of the deformation zone length to the blank diameter is 3.4:1). The compression-torsion composite plastic deformation formed by the spiral motion of the blank realizes ultra-large plastic deformation of the whole rolled piece with a cumulative area reduction rate of up to 73%.

[0009] However, the existing technology has the following limitations that need to be improved: the degree of grain refinement needs to be further improved to meet the requirements of higher performance. Summary of the invention

[0010] In view of the above problems, the purpose of the present invention is to provide a new method for ultrafine grain rolling in the subcritical zone of medium carbon steel bars by accumulating ultra-large torsional deformation in the subcritical zone of ferrite and pearlite.

[0011] The technical solution of the present invention is: the method for ultrafine grain rolling in the subcritical region of a medium carbon steel bar of the present invention comprises the following operating steps:

[0012] The first step is to design the deformation tool and determine the deformation parameters: using finite element simulation technology, establish a finite element model of medium carbon steel bars, and set the convergence condition as follows: the torsion angle of any particle in the deformation zone is not less than 180°, determine the shape of the roller and guide plate, as well as the roller surface cone angle α, feed angle β, rolling angle γ, hole ovality coefficient, roller pitch and other adjustment parameters;

[0013] If the torsion angle of the deformation tool meets the convergence condition, proceed to the next step. If it does not meet the convergence condition, repeat the first step until it meets the convergence condition.

[0014] The second step is the preparation and installation of deformation tools: design the curved roller and curved guide plate according to the determined optimal process parameters;

[0015] Design the rolling angle adjustment pads, design the feed angle adjustment tooling, and then complete the preparation, processing, installation and commissioning of the curved rollers, curved guide plates, rolling angle adjustment pads, and feed angle adjustment tooling;

[0016] The third step is to adjust the deformation parameters: after the installation and debugging is completed, adjust the parameters such as the roller surface cone angle α, feed angle β, rolling angle γ, hole ovality coefficient, roller pitch, etc. according to the optimal process parameters;

[0017] Step 4: Billet heating: Place billets with a diameter of 40-80 mm and a length of 400-1100 mm in a heating furnace and heat to 600-727°C. The heating time is calculated as t=D×(0.6-0.8)min, where D is the billet diameter in mm.

[0018] The fifth step is rolling test: the heated billet is transferred from the heating furnace to the guide trough of the rolling mill. The transfer time is 8s. The billet is fed through the guide trough and sent into the deformation zone between the rollers. The billet moves spirally in the deformation zone until the deformation is completed and completely leaves the deformation zone. The billet after rolling is air-cooled to room temperature (about 25°C).

[0019] Furthermore, when the billet is deformed during rolling, the billet is in a subcritical state of ferrite and pearlite.

[0020] Furthermore, in the fifth step, when the billet is rolled in the deformation zone, the feed angle β is greater than 24°, the rolling angle γ is greater than 18°, the roll speed n is less than 35 r / min, the cone angle α of the roll surface in the deformation zone is greater than 4°, and the ellipticity coefficient is less than 1.02.

[0021] Furthermore, in the fifth step, when the blank is rolled in the deformation zone, the area reduction rate is greater than 70%, and the roller surface is coarsened to a roughness greater than 6.4.

[0022] The beneficial effects of the present invention are: 1. The present invention can expand the degree of grain refinement and greatly improve material performance; 2. During the operation of the present invention, the relatively low temperature can reduce energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the operation flow of the present invention;

[0024] Figure 2 This is a schematic diagram of the original structure of the 45 steel bar in Example 1 of the present invention;

[0025] Figure 3 It is a schematic diagram of the structure of the 45 steel bar after rolling in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The specific technical solutions of the present invention are further described in detail below in conjunction with specific examples.

[0027] like Figure 1 As shown, a method for subcritical ultrafine grain rolling of a medium carbon steel bar according to the present invention comprises the following steps:

[0028] The first step is to design the deformation tool and determine the deformation parameters: using finite element simulation technology, establish a finite element model of medium carbon steel bars, and set the convergence condition as follows: the torsion angle of any particle in the deformation zone is not less than 180°, determine the shape of the deformation tools such as the roller and guide plate, as well as the roller surface cone angle α, feed angle β, rolling angle γ, hole ovality coefficient, roller spacing and other adjustment parameters;

[0029] If the torsion angle of the deformation tool meets the convergence condition, proceed to the next step. If it does not meet the convergence condition, repeat the first step until it meets the convergence condition.

[0030] The second step is the preparation and installation of deformation tools: according to the already determined, design the curved roller (and curved guide plate and other deformation tools;

[0031] Design the rolling angle adjustment pads, design the feed angle adjustment tooling, and then complete the preparation, processing, installation and commissioning of the curved rollers, curved guide plates, rolling angle adjustment pads, and feed angle adjustment tooling;

[0032] The third step is to adjust the deformation parameters: after the installation and debugging is completed, adjust the parameters such as the roller surface cone angle α, feed angle β, rolling angle γ, hole ovality coefficient, roller pitch, etc. according to the optimal process parameters;

[0033] Step 4: Billet heating: Place billets with a diameter of 40-80 mm and a length of 400-1100 mm in a heating furnace and heat to 600-727°C. The heating time is calculated as t=D×(0.6-0.8)min, where D is the billet diameter in mm.

[0034] The fifth step is rolling test: the heated billet is transferred from the heating furnace to the guide trough of the rolling mill. The transfer time is 8s. The billet is fed through the guide trough and sent into the deformation zone between the rollers. The billet moves spirally in the deformation zone until the deformation is completed and completely leaves the deformation zone. The billet after rolling is air-cooled to room temperature.

[0035] Furthermore, when the billet is deformed during rolling, the billet is in a subcritical state of ferrite and pearlite.

[0036] Furthermore, in the fifth step, when the billet is rolled in the deformation zone, the feed angle β is greater than 24°, the rolling angle γ is greater than 18°, the roll speed n is less than 35 r / min, the cone angle α of the roll surface in the deformation zone is greater than 4°, and the ellipticity coefficient is less than 1.02.

[0037] Furthermore, in the fifth step, when the blank is rolled in the deformation zone, the area reduction rate is greater than 70%, and the roller surface is coarsened to a roughness greater than 6.4.

[0038] Embodiment 1:

[0039] The exemplary embodiments of the present invention are described in detail below by specific examples. The following examples take 45 steel bars with a blank specification of 170×650 mm as an example, however, the present invention is not limited thereto, and 45 steel bars with other specifications can also be produced by the method of the present invention.

[0040] The production process of this example is as follows:

[0041] The purchased 45 steel bars are obtained by the manufacturer through smelting, forging and machining in a vacuum consumable arc furnace, and the quality meets the rolling requirements. The microstructure of each part of the cylindrical billet is evenly distributed, and no defects such as inclusions and pores are found.

[0042] The first step is to design the tool and determine the deformation parameters: First, the finite element model of 45 steel bar is established by using finite element simulation technology, and the convergence condition is set as follows: the torsion angle of any particle in the deformation zone is not less than 180°. When the roller surface cone angle α = 5°, the feed angle β = 24°, the rolling angle γ = 18°, the hole ellipticity coefficient = 1.01, and the roller spacing = 25mm, the torsion angle is calculated by finite element = 240°;

[0043] The second step is the preparation and installation of deformation tooling: according to the determined optimal process parameters, the roller and guide plate models are designed; the adjustment pads are designed, and then the preparation, processing, installation and commissioning of the rollers, guide plates and adjustment pads are completed; specifically, the adjustment pads, rolling angle and feed angle adjustment pads are unified as adjustment pads, and a total of four pads are fixed on the four legs respectively, and the rolling angle and feed angle are adjusted by adjusting the shape of the pads);

[0044] The third step is to adjust the deformation parameters: after the installation and debugging is completed, adjust the mill feed angle β = 24°, rolling angle γ = 18°, hole ovality coefficient = 1.01, and roller distance = 25mm according to the optimal process parameters (the pad is fixed to the bearing seat so that it will not shake during the operation);

[0045] Step 4: Billet heating: Place a 45 steel billet with a diameter of 50 mm and a length of 600 mm in a heating furnace and heat it to 700°C. The heating time is t = 50 min, where D is the billet diameter in mm.

[0046] The fifth step is rolling test: the heated billet is transferred from the heating furnace to the guide trough of the rolling mill. The transfer time is 8s. The billet is fed through the guide trough and sent into the deformation zone between the rollers. The roller speed is 30r / min. The billet spirally moves in the deformation zone until the deformation is completed and completely leaves the deformation zone. The surface reduction rate is 70%. The billet after rolling is air-cooled to room temperature.

[0047] The original organization Figure 2 As shown, the average grain size is 55 μm; after rolling using the present invention, the grain size of 45 steel is as shown in Figure 3 As shown, the grain size is about 0.8 μm and the grain refinement degree is 98.5%.

Claims

1. A method for rolling medium carbon steel bars in a subcritical region with ultrafine grains, characterized in that: The operation steps are as follows: Step (1): Design of deformation tool and determination of deformation parameters; Step (2): Deformation tool processing, preparation and installation; Step (3): deformation parameter adjustment; Step (4): heating the blank; Step (5): rolling test.

2. The method for rolling medium carbon steel bars in subcritical region ultrafine grains according to claim 1, characterized in that: In step (1), the deformation tool design and the determination of deformation parameters are specifically as follows: using finite element simulation technology, a finite element model of a medium carbon steel bar is established, and the convergence condition is set as follows: the torsion angle of any particle on the blank located in the deformation zone is not less than 180°, and the shapes of the rollers and guide plates, as well as the roller surface taper angle α, feed angle β, rolling angle γ, hole ovality coefficient, and roller spacing adjustment parameters are determined; If the torsion angle of the blank meets the convergence conditions under the determined deformation tool and roller surface cone angle α, feed angle β, rolling angle γ, hole type ovality coefficient, and roller spacing adjustment parameters, proceed to the next step. If the convergence conditions are not met, repeat the first step until the convergence conditions are met.

3. The method for rolling medium carbon steel bars in subcritical region ultrafine grains according to claim 1, characterized in that: In step (2), the deformation tool processing, preparation and installation are specifically: designing a curved roller and a curved guide plate according to the determined optimal process parameters; Design the rolling angle adjustment pads and feed angle adjustment tooling, and then complete the preparation, processing, installation and commissioning of curved rollers, curved guide plates, rolling angle adjustment pads and feed angle adjustment tooling.

4. The method for subcritical ultrafine grain rolling of medium carbon steel bars according to claim 1, characterized in that: In step (3), the deformation parameter adjustment is specifically: after the installation and debugging is completed, the parameters of the rolling mill roll surface cone angle α, feed angle β, rolling angle γ, hole type ovality coefficient and roll spacing are adjusted according to the optimal process parameters.

5. The method for subcritical ultrafine grain rolling of medium carbon steel bars according to claim 1, characterized in that: In step (4), the process of heating the blank is: placing the blank in a heating furnace for heating, and the heating time is calculated as t=D×(0.6-0.8) min, wherein D is the diameter of the blank, in mm.

6. The method for subcritical ultrafine grain rolling of medium carbon steel bars according to claim 5, characterized in that: The diameter of the blank is 40-80 mm, and the length is 400-1100 mm; the heating temperature is 600-727°C.

7. The method for subcritical ultrafine grain rolling of medium carbon steel bars according to claim 1, characterized in that: In step (5), the process of the rolling test is: the heated billet is transferred from the heating furnace to the rolling mill guide trough for a transfer time of 8 seconds, the billet is fed through the guide trough, and the billet is fed into the deformation zone between the rollers. The billet spirally moves in the deformation zone until the deformation is completed and completely leaves the deformation zone. The billet after rolling is air-cooled to room temperature.

8. The method for subcritical ultrafine grain rolling of medium carbon steel bars according to claim 1, characterized in that: In step (5), when the billet is deformed by rolling, the billet is deformed in the temperature range of ferrite and pearlite.

9. The method for subcritical ultrafine grain rolling of medium carbon steel bars according to claim 1, characterized in that: In step (5), when the blank is rolled in the deformation zone, the feed angle β is greater than 24°, the rolling angle γ is greater than 18°, the roll speed n is less than 35 r / min, the roll surface cone angle α in the deformation zone is greater than 4°, and the ellipticity coefficient is less than 1.

02.

10. The method for subcritical ultrafine grain rolling of medium carbon steel bars according to claim 9, characterized in that: When the blank is rolled in the deformation zone, the area reduction ratio ((original area - area after rolling) / original area) is greater than 70%, and the roller surface is coarsened to a roughness greater than 6.4.

Citation Information

Patent Citations

  • 3D-SPD forming method for large-size superfine pearlite medium carbon steel bars

    CN112044950A

  • 3D-SPD forming method for large-size superfine bainite medium carbon steel bars

    CN112044951A

  • 3D-SPD ultrafine grain bar forming method for F+P type non-quenched and tempered steel

    CN112044952A

  • Regulation and control method for carbide of large-size gun steel bar

    CN113430358A

  • High-toughness rolling method for large-size gun steel bar

    CN113430359A