Extrusion type printing process parameter design method based on rheological characteristics of biological materials

By analyzing the rheological properties of biomaterials and optimizing printing parameters, the problem of low filament diameter accuracy in 3D printing of biomaterials is solved, and high-precision tissue and organ construction is achieved.

CN118849418AActive Publication Date: 2024-10-29HARBIN INST OF TECH

Patent Information

Application Number
CN202411091646.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-29
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The rheological properties of materials are ignored in existing 3D printing of biomaterials, resulting in unsatisfactory printing parameters and low filament diameter accuracy, making it difficult to achieve high-precision tissue and organ structures.

Method used

By obtaining the complex modulus versus temperature curve and the viscosity versus shear rate curve of the polymer material, the optimal printing temperature and extrusion speed can be obtained through analysis and fitting, using 3D printing equipment that can control temperature and extrusion speed respectively. Experiment, record filament diameter data, build a prediction model to optimize printing parameters, and achieve high-precision printing of filaments.

Benefits of technology

It effectively improves the diameter accuracy of 3D printing filaments, reduces printing errors, and improves the accuracy and repeatability of tissue and organ construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118849418A_ABST
    Figure CN118849418A_ABST
Patent Text Reader

Abstract

The invention discloses an extrusion type printing process parameter design method based on rheological characteristics of a biological material, and relates to the technical field of additive materials. The problem that in existing biological material 3D printing, due to the fact that rheological characteristics of materials are neglected, obtained printing parameters are not ideal, and then the diameter precision of filaments is low is solved. The 3D printing device capable of controlling key parameters respectively is built, 3D printing of target materials under different parameters is achieved, the printing precision is recorded, a printing precision prediction model is built based on experimental data, the printing parameters are optimized, and filament printing with high diameter precision is completed. Rheology data are analyzed through a rheology test, and the optimal temperature and the optimal extrusion speed are determined; a 3D printing device capable of controlling the temperature and the extrusion speed respectively is built, and the relation between the printing precision and technological parameters in the printing process is explored. The method is used for additive printing of tissues or organs in transplantation surgery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a method for designing extrusion printing process parameters based on the rheological properties of biomaterials, which is used for 3D printing of human tissues and organs. Background Art

[0002] In the biomedical field, tissue engineering technology has become an important means of serving regenerative medicine. This technology uses healthy cells and biocompatible materials as raw materials to prepare tissues or organs that can be used in transplant surgery to alleviate the problem of insufficient donors. Since tissues and organs usually have complex three-dimensional structures, additive manufacturing technology represented by 3D printing technology has become the best means in the field of biomanufacturing.

[0003] The typical feature of this technology is that the material is extruded from the ink cartridge through a nozzle to construct a continuous filament with a diameter of several hundred microns, which is then deposited on the platform in a predetermined trajectory to construct a three-dimensional tissue and organ structure by stacking layers. Since most biological inks are high-molecular polymers with complex rheological properties, their unique viscoelasticity makes them have stringent requirements on the printing environment: when the temperature is high or the shear rate of the material is high, the material exhibits Newtonian viscosity, its viscosity decreases, and its fluidity increases, making the printed filaments poor in formability; when the temperature is low or the shear rate of the material is low, the material exhibits Hooke's elasticity, its viscosity is high, and its fluidity is poor, causing the printed filaments to undergo plastic deformation, resulting in filament expansion or even breakage.

[0004] In the 3D printing process, two printing parameters have a direct impact on the printing conditions: the temperature inside the print head affects the temperature to which the material is subjected; the extrusion speed affects the shear rate to which the material is subjected. Filament deformation caused by inappropriate printing parameters (temperature and extrusion speed) can lead to a large deviation between the actual filament diameter and the designed value, i.e., low filament diameter accuracy. As a basic component for constructing a three-dimensional structure, the error of the filament will be gradually magnified during the 3D printing process, causing huge errors in the overall structure, making it difficult to achieve tissue and organ construction with high accuracy.

[0005] At present, in order to obtain the ideal filament printing process parameters, the trial and error method is usually used to control the temperature and extrusion speed until the ideal filament diameter is obtained. In this process, the process parameters need to be adjusted repeatedly, which is not only time-consuming, but also lacks reliability and repeatability. The reason for this phenomenon is that the rheological properties of biomaterials are ignored, and the printing parameters are not designed according to the rheological characteristics of different materials. Therefore, in order to obtain the printing process parameters (temperature and extrusion speed) that can extrude ideal filaments, there is an urgent need for a method based on the rheological properties of biomaterials to guide the design of process parameters, and ultimately achieve the improvement of the printing accuracy of printed filaments.

[0006] In summary, in the existing 3D printing of biomaterials, due to the neglect of the rheological properties of the materials, the obtained printing parameters are not ideal, which leads to the problem of low filament diameter accuracy. Summary of the invention

[0007] The purpose of the present invention is to solve the problem of low filament diameter accuracy caused by ignoring the rheological properties of materials in existing biomaterial 3D printing, resulting in unsatisfactory printing parameters and thus providing a method for designing extrusion printing process parameters based on the rheological properties of biomaterials.

[0008] The technical solution of the present invention is:

[0009] A method for designing process parameters of extrusion printing based on the rheological properties of biomaterials comprises the following steps:

[0010] Step 1: Obtain the curve of the change of the complex modulus of the polymer material to be printed with temperature and the curve of the change of viscosity with shear rate at a certain temperature;

[0011] Step 2: Analyze the curve of the change of complex modulus with temperature to find the change law of the complex modulus of 3D printing materials with temperature;

[0012] Step 3: Under the most suitable 3D printing temperature obtained in step 2, analyze the curve of viscosity versus shear rate to find the law of viscosity variation of 3D printing materials versus shear rate;

[0013] Step 31: Convert the shear rate in viscosity-shear rate:

[0014]

[0015] in is the shear rate; v is the fluid extrusion velocity; d is the inner diameter of the pipe;

[0016] Step 32: Obtain the viscosity variation curve with 3D printing extrusion speed by converting the shear rate;

[0017] Step 33: Select the extrusion speed with low viscosity value for printing to ensure the smooth progress of 3D printing;

[0018] Step 4: Prepare 3D printing equipment that can control temperature and extrusion speed separately;

[0019] Step 5: Use a 3D printing device that can control the temperature and extrusion speed respectively to perform 3D printing of the target material at different temperatures and extrusion speeds, and record the filament diameter;

[0020] Step 6: Arrange the experimental data, use the temperature, extrusion speed and filament diameter data in different experimental groups as the coordinate values ​​of x, y, and z, respectively, and obtain a set of three-dimensional bar graphs;

[0021] The experimental data in the three-dimensional bar graph was imported into the analysis software, and the variation curve of the filament diameter under different temperatures and extrusion speeds was fitted to serve as a prediction model for controlling the filament diameter by adjusting the two printing parameters;

[0022] Step 7: Optimize printing parameters through prediction model:

[0023] Step 71: Determine the target printing filament diameter;

[0024] Step 72: Select appropriate temperature and extrusion speed in the surface of the prediction model according to the diameter as high-precision printing parameters of the target material;

[0025] Step 8: Perform 3D printing of the target material using the parameters selected in step 7-2, and verify the 3D printing accuracy.

[0026] Furthermore, in step 1, the method of obtaining the curve of the change of complex modulus with temperature and the curve of the change of viscosity with shear rate at a certain temperature is as follows;

[0027] Using a rotational rheometer with temperature control function, the target material is subjected to vibration temperature scanning analysis and testing to obtain the curve of complex modulus changing with temperature;

[0028] By conducting steady-state shear scanning analysis tests on the target material, the curve of viscosity changing with shear rate at a certain temperature is obtained.

[0029] Furthermore, in step 2, the analysis process of the curve diagram of the change of complex modulus with temperature is as follows:

[0030] Due to the particularity of polymer materials, their physical properties simultaneously reflect Newtonian viscosity and Hooke's elasticity, that is, polymer material viscoelasticity;

[0031] Complex modulus is a rheological property used to describe the viscoelasticity of polymer materials. It is divided into storage modulus G' and dissipation modulus G". Storage modulus G' is used to measure the Hookean elasticity of the material, and dissipation modulus G" is used to measure the Newtonian viscosity of the material.

[0032] When the storage modulus G' is greater than the dissipation modulus G", it means that the Hooke's elasticity of the polymer material is dominant, and the polymer material exhibits elasticity similar to that of a solid. At this time, the material fluidity is poor, causing plastic deformation of the printed filament, resulting in expansion and fracture of the filament.

[0033] When the storage modulus G' is smaller than the dissipation modulus G", it means that the Newtonian viscosity of the polymer material is dominant, and the polymer material exhibits liquid-like fluidity. At this time, the printed filament has weak molding ability.

[0034] Therefore, by analyzing the curve of complex modulus changing with temperature, it is concluded that as the temperature increases, the material gradually changes from solid to liquid. When the storage modulus G' and dissipation modulus G" curves intersect, the material has properties between solid and liquid.

[0035] Furthermore, the 3D printing equipment in step 4 that can control the temperature and extrusion speed respectively includes: a servo motor, a coupling, a lead screw, a lead screw nut, an L-shaped pressure plate, a nozzle push rod, a temperature-controlled printing nozzle and a frame; the frame is vertically arranged, the servo motor is vertically installed on the upper part of the frame, the output shaft of the servo motor is connected to one end of the lead screw located on the frame, the lead screw nut is installed on the lead screw, the vertical section of the L-shaped pressure plate is connected to the lead screw nut, the horizontal section of the L-shaped pressure plate is connected to the nozzle push rod, the nozzle push rod is inserted in the temperature-controlled printing nozzle, and the lifting and lowering of the polymer material in the temperature-controlled printing nozzle is realized under the follow-up movement of the L-shaped pressure plate.

[0036] Furthermore, the 3D printing equipment that can control the temperature and extrusion speed separately also includes a bearing seat, which is horizontally installed at the lower part of the frame, and the other end of the lead screw is installed in the bearing seat.

[0037] Preferably, the temperature-controlled printing nozzle has heating and cooling functions.

[0038] Furthermore, in step eight, the verification process of 3D printing accuracy is as follows:

[0039] Whether the 3D printing accuracy meets the requirements, if so, a 3D printing parameter design for improving the extruded filament diameter accuracy is completed;

[0040] If the requirements are not met, repeat step seven until the 3D printing accuracy meets the requirements. At this point, the 3D printing parameter design for improving the extruded filament diameter accuracy is completed.

[0041] Compared with the prior art, the present invention has the following effects:

[0042] 1. The present invention performs rheological tests on the target material and analyzes the rheological curve to obtain the optimal printing parameters. By building a 3D printing device that can control key parameters separately, 3D printing of the target material under different parameters is achieved and the printing accuracy is recorded. A printing accuracy prediction model is constructed based on experimental data and printing parameters are optimized to complete filament printing with high diameter accuracy.

[0043] 2. The present invention proposes a parameter optimization method that can achieve high-precision printing of 3D printing filaments. This design method can achieve high-precision printing of polymer filaments. The design process is simple and clear, and the efficiency of obtaining optimal parameters is high. It is of great significance for the high-precision in vitro construction of complex tissues and organs. Figures 1 to 7 As shown in the figure, through rheological tests, rheological data are analyzed to determine the optimal temperature and extrusion speed; by building a 3D printing device that can control the temperature and extrusion speed respectively, filaments are printed at different temperatures and extrusion speeds, and the diameter of the filaments is measured to explore the relationship between printing accuracy and process parameters during the printing process. The most commonly used polymer in biomanufacturing, poly (L-lactide-caprolactone) (PLCL), is used as the printing material to verify the feasibility of the designed method: Figure 5 The following is the result of the printing experiment. The experimental results were analyzed by computer and fitted as follows: Figure 6 The prediction model shown in Figure 2 is used to select the parameters based on the prediction model and conduct filament printing experiments. Finally, the Figure 7 The diameter accuracy of the filament shown is within 5μm. When this method is not used, the absolute error of the diameter of the printed PLCL filament can reach 22μm. After using this method, the absolute error of the filament is reduced by 77.3%, effectively improving the diameter accuracy of the 3D printed filament. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a flow chart of a three-dimensional printing parameter design method for improving the diameter accuracy of extruded filaments of the present invention;

[0045] Figure 2 This is the structural diagram of the designed extrusion 3D printing device;

[0046] Figure 3 is the complex modulus-temperature curve of PLCL;

[0047] Figure 4 This is the viscosity-shear rate curve of PLCL at the optimum printing temperature;

[0048] Figure 5 is the diameter of 3D printed PLCL filaments at different temperatures and extrusion speeds;

[0049] Figure 6 It is the PLCL filament accuracy prediction model under different temperatures and extrusion speeds;

[0050] Figure 7 It is a high-precision PLCL filament with different diameters;

[0051] Figure 8 This is the viscosity-extrusion speed curve of PLCL.

[0052] Among them: 1. servo motor, 2. coupling, 3. lead screw, 4. lead screw nut, 5. L-shaped pressure plate, 6. nozzle push rod, 7. temperature-controlled printing nozzle, 8. frame. DETAILED DESCRIPTION

[0053] Specific implementation method 1: Combination Figures 1 to 8 To illustrate this embodiment, the embodiment includes the following steps:

[0054] Step 1: Obtain the curve of the change of complex modulus with temperature and the curve of the change of viscosity with shear rate at a certain temperature of the polymer material to be printed; wherein "a certain temperature" is the temperature value near the intersection of the storage modulus G' and the dissipation modulus G" curve in the complex modulus-temperature curve;

[0055] Step 2: Analyze the curve of the change of complex modulus with temperature to find the change law of the complex modulus of 3D printing materials with temperature;

[0056] Step 3: Under the most suitable 3D printing temperature obtained in step 2, analyze the curve of viscosity versus shear rate to find the law of viscosity variation of 3D printing materials versus shear rate;

[0057] Step 31: Convert the shear rate in viscosity-shear rate:

[0058]

[0059] in is the shear rate; v is the fluid extrusion velocity; d is the inner diameter of the pipe;

[0060] Since the 3D printing process is driven by the screw pushing the nozzle push rod, the cross-sectional area of ​​the push rod and the cross-sectional area of ​​the nozzle are converted to obtain: for the fluid in the pipeline: A1 / A2=V2 / V1; where A is the area at the cross section, and V is the flow rate at the cross section;

[0061] Step 32: Obtain the viscosity variation curve with 3D printing extrusion speed by converting the shear rate;

[0062] Step 33: Select the extrusion speed with low viscosity value for printing to ensure the smooth progress of 3D printing;

[0063] When the viscosity value is low, it means that the viscosity curve decreases sharply as the shear rate increases, then the rate of decrease slows down, and finally remains almost unchanged. The viscosity value taken here is the value when the viscosity remains almost unchanged. Figure 4 The viscosity value of the middle finger is less than 80000mPas;

[0064] Step 4: Prepare 3D printing equipment that can control temperature and extrusion speed separately;

[0065] Step 5: Use a 3D printing device that can control the temperature and extrusion speed respectively to perform 3D printing of the target material at different temperatures and extrusion speeds, and record the filament diameter;

[0066] Step 6: Arrange the experimental data, use the temperature, extrusion speed and filament diameter data in different experimental groups as the coordinate values ​​of x, y, and z, respectively, and obtain a set of three-dimensional bar graphs;

[0067] The experimental data in the three-dimensional bar graph is imported into Origin or Excel analysis software, and the variation curve of the filament diameter under different temperatures and extrusion speeds is obtained by fitting, which is used as a prediction model for controlling the filament diameter by adjusting the two printing parameters;

[0068] Step 7: Optimize printing parameters through prediction model:

[0069] Step 71: Determine the target printing filament diameter;

[0070] Step 72: According to the diameter, select the appropriate temperature and extrusion speed in the surface of the prediction model as the high-precision printing parameters of the target material; the appropriate temperature is: according to the target printing filament diameter in step 71, select the point where the diameter is located in the prediction surface, and find the corresponding temperature and extrusion speed parameters;

[0071] Step 8: Perform 3D printing of the target material using the parameters selected in step 7-2, and verify the 3D printing accuracy.

[0072] Specific implementation method 2: Combination Figure 3 To illustrate this embodiment, in step 1 of this embodiment, the method of obtaining the curve of the change of complex modulus with temperature and the curve of the change of viscosity with shear rate at a certain temperature is as follows;

[0073] Using a rotational rheometer with temperature control function, the target material is subjected to vibration temperature scanning analysis and testing to obtain the curve of complex modulus changing with temperature;

[0074] By conducting steady-state shear scanning analysis tests on the target material, the curve of viscosity changing with shear rate at a certain temperature is obtained.

[0075] Such an arrangement facilitates providing necessary data support for the subsequent determination of the temperature and extrusion speed of the polymer material. Other components and connection relationships are the same as those in the first specific embodiment.

[0076] Specific implementation method three: Combination Figure 3-Figure 6 To illustrate this embodiment, the analysis process of the curve diagram of the change of complex modulus with temperature in step 2 of this embodiment is as follows:

[0077] Due to the particularity of polymer materials, their physical properties simultaneously reflect Newtonian viscosity and Hooke's elasticity, that is, polymer material viscoelasticity;

[0078] Complex modulus is a rheological property used to describe the viscoelasticity of polymer materials. It is divided into storage modulus G' and dissipation modulus G". Storage modulus G' is used to measure the Hookean elasticity of the material, and dissipation modulus G" is used to measure the Newtonian viscosity of the material.

[0079] When the storage modulus G' is greater than the dissipation modulus G", it means that the Hooke's elasticity of the polymer material is dominant, and the polymer material exhibits elasticity similar to that of a solid. At this time, the material fluidity is poor, causing plastic deformation of the printed filament, resulting in expansion and fracture of the filament.

[0080] When the storage modulus G' is smaller than the dissipation modulus G", it means that the Newtonian viscosity of the polymer material is dominant, and the polymer material exhibits liquid-like fluidity. At this time, the printed filament has weak molding ability.

[0081] Therefore, by analyzing the curve of complex modulus changing with temperature, it is concluded that as the temperature increases, the material gradually changes from solid to liquid. When the storage modulus G' and dissipation modulus G" curves intersect, the material has properties between solid and liquid.

[0082] Such an arrangement facilitates accurate determination of the optimum printing temperature. Other components and connection relationships are the same as those of the first or second specific implementation.

[0083] Specific implementation method four: Combination Figure 2 The present embodiment is described. The 3D printing equipment capable of controlling the temperature and the extrusion speed respectively in step 4 of the present embodiment comprises: a servo motor 1, a coupling 2, a lead screw 3, a lead screw nut 4, an L-shaped pressing plate 5, a nozzle push rod 6, a temperature-controlled printing nozzle 7 and a frame 8;

[0084] The frame 8 is vertically arranged, and the servo motor 1 is vertically installed on the upper part of the frame 8. The output shaft of the servo motor 1 is connected to one end of the lead screw 3 located on the frame 8, and the lead screw nut 4 is installed on the lead screw 3. The vertical section of the L-shaped pressing plate 5 is connected to the lead screw nut 4, and the horizontal section of the L-shaped pressing plate 5 is connected to the nozzle push rod 6. The nozzle push rod 6 is inserted in the temperature-controlled printing nozzle 7, and the lifting and lowering of the polymer material in the temperature-controlled printing nozzle 7 is realized under the follow-up movement of the L-shaped pressing plate 5.

[0085] In this way, since the extrusion printing process parameter design method based on the rheological properties of biomaterials of the present invention can achieve the best printing accuracy, it is necessary to have a device that can accurately control the temperature and the accurate printing speed. In this embodiment, the printing temperature is regulated by the temperature-controlled printing nozzle 7, and the screw nut 4 moves up and down on the screw 3, driving the L-shaped pressing plate 5 and the nozzle push rod 6 to rise and fall, thereby achieving the regulation of the extrusion speed. The other components and connection relationships are the same as any one of the specific embodiments one to three.

[0086] Specific implementation method five: Combination Figure 2 To illustrate this embodiment, the 3D printing equipment capable of separately controlling the temperature and the extrusion speed of this embodiment further comprises a bearing seat, which is horizontally mounted at the lower portion of the frame 8, and the other end of the lead screw 3 is mounted in the bearing seat.

[0087] Such arrangement facilitates the smooth rotation of the lead screw 3 and ensures the accuracy of the lifting and lowering of the lead screw nut 4. Other components and connection relationships are the same as any one of the specific implementation modes 1 to 4.

[0088] Specific implementation method six: Combination Figure 2 To explain this embodiment, the temperature-controlled printing nozzle 7 of this embodiment has heating and cooling functions.

[0089] With such arrangement, the heating function in this embodiment includes but is not limited to the resistance wire and the heating rod, and the cooling function includes but is not limited to the cooling sheet, which is flexible and convenient to use, and can mainly achieve fast and accurate temperature control. The other components and connection relationships are the same as any one of the specific embodiments 1 to 5.

[0090] Specific implementation method seven: Combination Figure 1 To illustrate this embodiment, in step eight of this embodiment, the verification process of 3D printing accuracy is as follows:

[0091] Whether the 3D printing accuracy meets the requirements, if so, a 3D printing parameter design for improving the extruded filament diameter accuracy is completed;

[0092] If the requirements are not met, repeat step seven until the 3D printing accuracy meets the requirements. At this point, the 3D printing parameter design for improving the extruded filament diameter accuracy is completed.

[0093] With such arrangement, the accuracy and quality of the printed filaments are ensured to be optimal through verification. The other components and connection relationships are the same as any one of the specific embodiments 1 to 6.

[0094] Combination Figures 1 to 7 The working process of the present invention is described:

[0095] The above invention object is achieved through the following technical solutions:

[0096] Step 1: Use a rotational rheometer with temperature control function to perform vibration temperature scanning analysis and test on the target material to obtain the curve of the change of complex modulus with temperature; perform steady-state shear scanning analysis and test on the target material to obtain the curve of the change of viscosity with shear rate at a certain temperature.

[0097] Step 2: Analyze the curve of the change of complex modulus with temperature to find the most suitable temperature for 3D printing. Due to the particularity of polymer materials, they often reflect Newtonian viscosity and Hooke's elasticity in physical properties, that is, polymer material viscoelasticity. Complex modulus is a rheological property used to describe the viscoelasticity of polymer materials, which is divided into storage modulus (G') and dissipation modulus (G"). Among them, storage modulus is used to measure the Hooke's elasticity of the material, and dissipation modulus is used to measure the Newtonian viscosity of the material. When G' is greater than G", the Hooke's elasticity of the material is dominant, and the material exhibits elasticity similar to that of a solid. At this time, the material has poor fluidity, causing plastic deformation of the printed filaments, resulting in expansion and fracture of the filaments; when G' is less than G", the Newtonian viscosity of the material is dominant, and the material exhibits fluidity similar to that of a liquid. At this time, the printed filaments have weak molding ability. Therefore, by analyzing the curve of the complex modulus changing with temperature, it is concluded that as the temperature increases, the material gradually changes from a solid to a liquid. When the storage modulus G' and the dissipation modulus G" curves intersect, the material has properties between solid and liquid.

[0098] Step 3: Analyze the viscosity versus shear rate curve at the most suitable 3D printing temperature obtained in step 2. Polymer materials are composed of long-chain macromolecular clusters with variable volumes. When they are squeezed into the circular flow channel in the 3D printing nozzle, they usually experience shear thinning. That is, when the extrusion speed increases, the shear rate increases. At this time, the long-chain macromolecular clusters inside the material deform along the flow direction of the fluid, increasing the flow rate and ultimately reducing the apparent viscosity of the material. Therefore, by converting the shear rate in the viscosity-shear rate, we can obtain a curve of viscosity versus 3D printing extrusion speed. Select the extrusion speed with a lower viscosity value for printing to ensure smooth 3D printing. According to polymer fluid dynamics, the shear rate and extrusion speed inside the circular tube are converted as follows:

[0099]

[0100] in is the shear rate; v is the fluid extrusion velocity; d is the inner diameter of the pipe.

[0101] Step 4: Develop a new 3D printing device that can control temperature and extrusion speed separately. The mechanical structure of the device is as follows: Figure 2As shown, its components include: 1-servo motor, 2-coupling, 3-screw, 4-screw nut, 5-L-shaped pressure plate, 6-nozzle push rod, 7-temperature controlled printing nozzle. Its connection relationship is: 1. The motor shaft at the lower end of the servo motor is connected to the 3 screw through the 2 coupling, 4 screw nut is installed on the outside of the screw, 5-the upper end of the L-shaped pressure plate is connected to the screw nut, 5-the lower end of the L-shaped pressure plate is connected to the top of the 6 nozzle push rod, and the 6 nozzle push rod is inserted into the channel inside the 7 temperature controlled printing nozzle and can move up and down. The above-mentioned connection methods include but are not limited to threaded connection, welding, pin connection, etc.; 7 The temperature control shell can be heated or cooled: the heating method includes but is not limited to heating rods, electric heating wires, etc., and the cooling method includes but is not limited to cooling sheets, etc. Its working process is: the target material is loaded into the 7 temperature controlled printing nozzle, and the temperature of the printing nozzle is adjusted through the internal temperature control system, thereby controlling the temperature of the target material. Then, by controlling the rotation of servo motor 1, the rotation is transmitted to lead screw 3, and the meshing between lead screw 3 and lead screw 4 is used to control the reciprocating up and down motion of 5-L-shaped pressing plate at a fixed speed. The target material is extruded to achieve 3D printing of filaments.

[0102] Step 5: Use the printing equipment to perform 3D printing of the target material at different temperatures and extrusion speeds, and record the filament diameter;

[0103] Step 6: Organize the experimental data, use the temperature, extrusion speed and filament diameter data in different experimental groups as the coordinate values ​​of x, y, and z, and obtain a set of three-dimensional bar graphs. Import the experimental data in the figure into the analysis software, and fit the change surface of the filament diameter under different temperatures and extrusion speeds as a prediction model for controlling the filament diameter by adjusting the two printing parameters;

[0104] Step 7: The prediction model can be used to optimize the printing parameters: first determine the target printing filament diameter, and then select the appropriate temperature and extrusion speed in the surface of the prediction model according to the diameter as the high-precision filament printing parameters of the target material;

[0105] Step 8: By using the parameters to perform 3D printing on the target material, it is determined whether the printing accuracy meets the requirements, thus completing the verification of a 3D printing parameter design method for improving the accuracy of the extruded filament diameter.

[0106] Example:

[0107] Printing material: A biodegradable polymer, poly-L-lactide-caprolactone (PLCL):

[0108] The purchased PLCL granular material was placed in a rotational rheometer and the complex modulus-temperature curve of PLCL was obtained using the oscillation temperature scanning analysis mode ( Figure 3 );

[0109] According to the obtained curve, it is found that the material exhibits solid properties at low temperatures and liquid properties at high temperatures. It is more suitable to print at 130℃-137℃. In order to further understand the characteristics of the material viscosity changing with the extrusion speed, the temperature at the intersection of the G' and G" curves: 134.5℃ is selected as the printing temperature, and a steady-state shear scanning analysis is performed to obtain the material viscosity changing with the shear rate curve ( Figure 4 ).

[0110] According to the obtained curve and the print head diameter used in the 3D printing experiment is 100μm, the material viscosity versus extrusion speed curve is obtained by conversion ( Figure 8 ), and determined that when the extrusion speed changes between 1.2 and 2.5 mm / s, the viscosity changes more steadily, which is a more appropriate 3D printing speed;

[0111] According to the above conclusions, 130, 134.5, and 137 °C were selected as temperature parameters; 1.2, 1.7, and 2.2 mm / s were selected as extrusion speed parameters. Printing experiments were carried out based on the proposed 3D printing equipment. The diameters of the printed filaments will be recorded in the future. Figure 5 Inside.

[0112] By fitting Figure 6 The surface in the figure can be used to obtain the extrusion speed and temperature parameters corresponding to different target filament diameters. Select different temperature parameters and print to obtain Figure 7 The printed filaments shown in the figure were used, and the printing accuracy of the filaments was measured. The final accuracy was controlled within 5μm, verifying the feasibility.

[0113] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for designing process parameters of extrusion printing based on the rheological properties of biomaterials, characterized by: It includes the following steps: Step 1: Obtain the curve of the change of the complex modulus of the polymer material to be printed with temperature and the curve of the change of viscosity with shear rate at a certain temperature; Step 2: Analyze the curve of the change of complex modulus with temperature to find the change law of the complex modulus of 3D printing materials with temperature; Step 3: Under the most suitable 3D printing temperature obtained in step 2, analyze the curve of viscosity versus shear rate to find the law of viscosity variation of 3D printing materials versus shear rate; Step 31: Convert the shear rate in viscosity-shear rate: in is the shear rate; v is the fluid extrusion velocity; d is the inner diameter of the pipe; Step 32: Obtain the viscosity variation curve with 3D printing extrusion speed by converting the shear rate; Step 33: Select Print at the extrusion speed when the viscosity value is low to ensure the smooth progress of 3D printing; Step 4: Prepare 3D printing equipment that can control temperature and extrusion speed separately; Step 5: Use a 3D printing device that can control the temperature and extrusion speed respectively to perform 3D printing of the target material at different temperatures and extrusion speeds, and record the filament diameter; Step 6: Arrange the experimental data, use the temperature, extrusion speed and filament diameter data in different experimental groups as the coordinate values ​​of x, y, and z, respectively, and obtain a set of three-dimensional bar graphs; The experimental data in the three-dimensional bar graph was imported into the analysis software, and the variation curve of the filament diameter under different temperatures and extrusion speeds was fitted to serve as a prediction model for controlling the filament diameter by adjusting the two printing parameters; Step 7: Optimize printing parameters through prediction model: Step 71: Determine the target printing filament diameter; Step 72: Select appropriate temperature and extrusion speed in the surface of the prediction model according to the diameter as high-precision printing parameters of the target material; Step 8: Perform 3D printing of the target material using the parameters selected in step 7-2, and verify the 3D printing accuracy.

2. The method for designing process parameters of extrusion printing based on the rheological properties of biomaterials according to claim 1, characterized in that: In step 1, the method of obtaining the curve of the change of complex modulus with temperature and the curve of the change of viscosity with shear rate at a certain temperature is as follows; Using a rotational rheometer with temperature control function, the target material is subjected to vibration temperature scanning analysis and testing to obtain the curve of complex modulus changing with temperature; By conducting steady-state shear scanning analysis tests on the target material, the curve of viscosity changing with shear rate at a certain temperature is obtained.

3. The method for designing process parameters of extrusion printing based on the rheological properties of biomaterials according to claim 1, characterized in that: The analysis process of the complex modulus versus temperature curve in step 2 is as follows: Due to the particularity of polymer materials, their physical properties simultaneously reflect Newtonian viscosity and Hooke's elasticity, that is, polymer material viscoelasticity; Complex modulus is a rheological property used to describe the viscoelasticity of polymer materials. It is divided into storage modulus G' and dissipation modulus G". Storage modulus G' is used to measure the Hookean elasticity of the material, and dissipation modulus G" is used to measure the Newtonian viscosity of the material. When the storage modulus G' is greater than the dissipation modulus G", it means that the Hooke's elasticity of the polymer material is dominant, and the polymer material exhibits elasticity similar to that of a solid. At this time, the material fluidity is poor, causing plastic deformation of the printed filament, resulting in expansion and fracture of the filament. When the storage modulus G' is smaller than the dissipation modulus G", it means that the Newtonian viscosity of the polymer material is dominant, and the polymer material exhibits liquid-like fluidity. At this time, the printed filament has weak molding ability. Therefore, by analyzing the curve of complex modulus changing with temperature, it is concluded that as the temperature increases, the material gradually changes from solid to liquid. When the storage modulus G' and dissipation modulus G" curves intersect, the material has properties between solid and liquid.

4. The method for designing process parameters of extrusion printing based on the rheological properties of biomaterials according to claim 3, characterized in that: The 3D printing equipment capable of controlling temperature and extrusion speed respectively in step 4 comprises: a servo motor (1), a coupling (2), a lead screw (3), a lead screw nut (4), an L-shaped pressing plate (5), a nozzle push rod (6), a temperature-controlled printing nozzle (7) and a frame (8); The frame (8) is arranged vertically, the servo motor (1) is vertically mounted on the upper part of the frame (8), the output shaft of the servo motor (1) is connected to one end of a lead screw (3) located on the frame (8), the lead screw nut (4) is mounted on the lead screw (3), the vertical section of the L-shaped pressing plate (5) is connected to the lead screw nut (4), the horizontal section of the L-shaped pressing plate (5) is connected to the nozzle push rod (6), the nozzle push rod (6) is inserted into the temperature-controlled printing nozzle (7), and is lifted and lowered under the follow-up movement of the L-shaped pressing plate (5) to extrude the polymer material in the temperature-controlled printing nozzle (7).

5. The method for designing extrusion printing process parameters based on the rheological properties of biomaterials according to claim 4, characterized in that: The 3D printing equipment capable of controlling the temperature and the extrusion speed respectively further comprises a bearing seat, which is horizontally mounted at the lower part of the frame (8), and the other end of the lead screw (3) is mounted in the bearing seat.

6. The method for designing process parameters of extrusion printing based on the rheological properties of biomaterials according to claim 5, characterized in that: The temperature-controlled printing nozzle (7) has heating and cooling functions.

7. The method for designing process parameters of extrusion printing based on the rheological properties of biomaterials according to claim 6, characterized in that: In step eight, the verification process for 3D printing accuracy is as follows: Whether the 3D printing accuracy meets the requirements, if so, a 3D printing parameter design for improving the extruded filament diameter accuracy is completed; If the requirements are not met, repeat step seven until the 3D printing accuracy meets the requirements. At this point, the 3D printing parameter design for improving the extruded filament diameter accuracy is completed.

Citation Information

Patent Citations

  • Hydrogel 3D printing material and preparation method thereof

    CN108359143A

  • Continuous functionally graded material and structure integrated manufacturing 3D printing device and method

    CN112895441A

  • Shape prediction method of extrusion type 3D printing bio-ink extrusion filament

    CN113554743A

  • Preparation method of 3D printing bio-ink material with controllable material distribution and preparation method of three-dimensional bionic hydrogel scaffold

    CN114470328A

  • System determining mechanical and-or rheological material properties of test body

    DE19644094A1

Cited By

  • Direct writing line morphology regulation and control method, device and equipment based on three-dimensional phase diagram and medium

    CN121572602A

  • Three-dimensional phase diagram-based direct writing line morphology regulation method and device, equipment and medium

    CN121572602B