Preparation method of PA (Polyamide) membrane taking PVDF (Polyvinylidene Fluoride) dendritic fiber membrane as supporting layer

By forming a polyamide film on a PVDF dendritic nanofiber membrane, the problems of low porosity and poor chemical resistance of the polyamide TFC membrane are solved, high water permeability flux and high rejection rate are achieved, and its application in sewage treatment and seawater is expanded. Application range in fade.

CN118849554AInactive Publication Date: 2024-10-29ANHUI POLYTECHNIC UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410875385.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polyamide TFC membranes have low porosity, poor inter-pore connectivity, and insufficient mechanical strength and chemical corrosion resistance, which limits their application in seawater desalination and sewage treatment.

Method used

A PVDF dendritic nanofiber membrane was prepared by high-voltage electrospinning as a supporting layer, and an ultra-thin polyamide film was formed on its surface through interfacial polymerization to form a polyamide film composite membrane with the PVDF dendritic nanofiber membrane as the middle layer.

Benefits of technology

It increases water permeability flux and interception rate, enhances mechanical strength and chemical resistance, expands the use scope of polyamide film composite membranes, effectively treats sewage and reduces secondary pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118849554A_ABST
    Figure CN118849554A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a PA (Polyamide) membrane taking a PVDF (Polyvinylidene Fluoride) dendritic fiber membrane as a supporting layer, and relates to the technical field of textile materials.The specific preparation method comprises the following steps: S1, preparing PVDF dendritic nanofibers; s2, performing hot pressing on the PVDF dendritic nanofiber membrane prepared in the step S1; s3, performing interfacial polymerization on the fiber membrane obtained in the step S2 to form a polyamide membrane; and S4, transferring the multi-layer membrane in the step S3 into a drying oven for post-treatment to obtain the PA membrane taking the PVDF dendritic fiber membrane as the supporting layer. The dendritic nanofiber membrane is adopted as a middle layer, the polyamide membrane is formed on the surface of the dendritic nanofiber membrane through polymerization of m-phenylenediamine and s-tribenzoyl chloride, then the polyamide membrane composite membrane is obtained through drying aftertreatment, and the polyamide membrane composite membrane is high in filtering efficiency, high in water permeation amount, wide in application range and capable of being applied to the fields of sewage treatment, seawater desalination and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile materials, and more specifically, to a method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer. Background Art

[0002] With the progress of society, the development of urbanization and the surge in global population, people's demand for clean water resources is surging, but global fresh water resources are becoming increasingly scarce. Therefore, in order to cope with environmental changes, shortage of fresh water resources and strict emission standards, it is urgent to find a method that can be used sustainably and effectively to obtain clean water. Wastewater treatment and seawater desalination are currently effective methods for obtaining clean water, and are also research focuses and hotspots in the field of environmental protection. In the past few decades, with the development of polymer membrane technology, membrane separation methods have dominated the water treatment process. At present, the most commonly used membrane in seawater desalination and sewage treatment is polyamide TFC membrane.

[0003] The most commonly used polyamide TFC membrane is composed of a PET nonwoven fabric bottom layer, a polysulfone or polyethersulfone ultrafiltration middle layer and a polyamide retention layer. Among them, polysulfone and polyethersulfone cast ultrafiltration membranes are dominant as middle layers in nanofiltration and reverse osmosis thin film composite membranes. However, the low porosity of polysulfone and polyethersulfone ultrafiltration membranes and the poor interconnectivity between pores make it difficult to effectively improve the permeation flux of the formed composite membrane water. In addition, the relatively low mechanical strength and poor chemical corrosion resistance of polysulfone and polyethersulfone further limit the scope of use of the composite membrane.

[0004] PVDF dendritic nanofiber membrane has a unique structure consisting of ultrafine branch fibers and trunk fibers, with high specific surface area, porosity and interconnected porous structure. Ultrafine branch fibers can effectively reduce the pore size on the surface of the fiber membrane. In addition, ultrafine branch fibers can form direct water channels with the polyamide layer during interfacial polymerization. This unique structure can give it the potential for application in polyamide thin film composite membranes.

[0005] The literature (Thin-film nanofibrous composite reverse osmosis membranes for Desalination and Highly Permeable Polymer Membranes Containing Directed Channels for Water Purification) discloses a thin film composite nanofiber membrane, which uses a composite middle layer of polyacrylonitrile nanofiber membrane as the bottom layer and ultrafine cellulose nanofiber as the top layer to prepare a polyamide thin film composite membrane with high retention rate and high water flux. Although this composite middle layer effectively reduces the pore size of the PAN nanofiber membrane, the operation of uniformly settling the ultrafine cellulose nanofiber in PAN is difficult, and the bonding force between the cellulose fiber and the PAN fiber membrane is limited.

[0006] Patent CN205951427U discloses a multi-layer composite structure polyamide film, which is a transition layer formed by coating nanocellulose and polyelectrolyte on a porous support layer substrate through a layer-by-layer assembly method, and then forming a polyamide layer through interfacial polymerization. This method is complex and difficult to operate.

[0007] Therefore, in order to solve the above technical problems, the present application proposes a method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer. Summary of the invention

[0008] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer.

[0009] To achieve the above object, the present invention provides the following technical solution: a method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer, comprising the following steps;

[0010] S1: Preparation of PVDF dendritic nanofiber membrane by high-voltage electrospinning method;

[0011] S2: hot pressing the PVDF dendritic nanofiber membrane prepared in S1;

[0012] S3: fixing the PVDF dendritic nanofiber membrane obtained in S2 on a glass plate, using m-phenylenediamine and tribenzoyl chloride to form an ultra-thin polyamide film on the surface of the PVDF dendritic nanofiber membrane by an interfacial polymerization method, thereby forming a polyamide film composite membrane with the PVDF dendritic nanofiber membrane as an intermediate layer;

[0013] S4: The polyamide film composite membrane with the PVDF dendritic nanofiber membrane as the middle layer obtained in S3 is rinsed with deionized water, and then placed in an oven for drying to obtain a PA membrane with the PVDF dendritic nanofiber membrane as the middle layer.

[0014] In this scheme, the electrospinning parameters in the high-voltage electrospinning method in S1 are: the spinning voltage is between 20 kv and 40 kv, the receiving distance is between 10 cm and 20 cm, and the drum speed is between 90 r / min and 110 r / min.

[0015] In this embodiment, the diameter of the fiber trunk in the PVDF dendritic nanofiber membrane prepared in S1 is between 100 nm and 500 nm, and the diameter of the branched fibers is between 5 nm and 100 nm.

[0016] It should be noted that the setting parameters of the hot pressing treatment in S2 are: pressure between 10MPa and 20MPa, temperature between 160°C and 180°C, and hot pressing time between 40min and 50min.

[0017] Furthermore, in the process of interfacial polymerization using the interfacial polymerization method in S3, the mass fraction of m-phenylenediamine is between 0.10wt% and 0.20wt%, and the mass fraction of tribenzoyl chloride is between 1wt% and 3wt%.

[0018] Among them, the specific operation of the interfacial polymerization method is: fix the hot-pressed PVDF dendritic nanofiber membrane on a glass plate, immerse the fixed membrane in a 2wt% m-phenylenediamine aqueous solution for 5 minutes, then take it out for surface drying, and then contact it with a 0.15wt% n-hexane solution for 2 minutes, and finally obtain the PATFC membrane through drying post-treatment.

[0019] Among them, in S4, the polyamide film with the PVDF dendritic nanofiber membrane as the middle layer is placed in an oven for drying, and the parameters set in the process are: the drying temperature is between 60° C. and 80° C., and the time is between 5 min and 15 min.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. In the present invention, a PVDF dendritic nanofiber membrane produced by high-voltage electrospinning is applied as an intermediate layer to a polyamide thin film composite membrane, and the advantages of the PVDF dendritic nanofiber membrane such as high porosity, high specific surface area and high proportion of interconnected pores are utilized to prepare a novel thin film composite membrane, which can obtain a high water permeation flux and maintain an extremely high retention rate;

[0022] 2. In the present invention, by using PVDF dendritic nanofiber membrane as the middle layer, PVDF has good mechanical strength and chemical resistance, and can effectively expand the application range of the polyamide film composite membrane.

[0023] 3. In the present invention, the polyamide composite membrane can effectively treat sewage, protect the environment, and solve the problem of secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0025] Figure 1 is a flow chart of the preparation process of the present invention;

[0026] Figure 2 The morphology of the PVDF nanofiber membrane in the present invention;

[0027] Figure 3 It is a schematic diagram of interfacial polymerization in the present invention;

[0028] Figure 4 Schematic diagram of the structure of the polyamide film composite dendritic nanofiber membrane in the present invention;

[0029] Figure 5 is a morphology diagram of the polyamide film in the present invention; (c1) and (c2) are SEM images at two different magnifications. DETAILED DESCRIPTION

[0030] To solve the above problems, the present invention provides a method for preparing a PA membrane with a PVDF dendritic fiber membrane as a support layer, wherein the PVDF dendritic nanofiber membrane is prepared by a high-voltage electrospinning method to prepare a fiber membrane with a branch-like and trunk-like structure, and then a polyamide film is formed on its surface by interfacial polymerization, thereby obtaining a polyamide TFC membrane. The ultimate purpose of the present invention is to prepare a thin film composite membrane with a high rejection rate and a high water flux.

[0031] The present invention adopts the dendritic nanofiber membrane as the middle porous support layer, which effectively increases the porosity and connectivity of the middle layer and significantly reduces the transmission resistance of water molecules.

[0032] The terms and abbreviations that require special attention in this manual are: metaphenylenediamine (MPD), tris-benzoyl chloride (TMC), polyvinylidene fluoride (PVDF), tetrabutylammonium chloride (TBAC), PET nonwoven fabric substrate, N,N-dimethylformamide (DMF), acetone, PVDF dendritic fiber membrane

[0033] Embodiment 1

[0034] like Figure 1-5 As shown, the present invention provides a method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer, comprising the following steps:

[0035] S1: Preparation of PVDF dendritic nanofiber membrane by high-voltage electrospinning method;

[0036] S2: hot pressing the PVDF dendritic nanofiber membrane prepared in S1;

[0037] S3: fixing the PVDF dendritic nanofiber membrane obtained in S2 on a glass plate, using m-phenylenediamine and tribenzoyl chloride to form an ultra-thin polyamide film on the surface of the PVDF dendritic nanofiber membrane by an interfacial polymerization method, thereby forming a polyamide film composite membrane with the PVDF dendritic nanofiber membrane as an intermediate layer;

[0038] S4: The polyamide film composite membrane with the PVDF dendritic nanofiber membrane as the middle layer obtained in S3 is rinsed with deionized water, and then placed in an oven for drying to obtain a PA membrane with the PVDF dendritic nanofiber membrane as the middle layer.

[0039] The electrospinning parameters in the S1 medium and high voltage electrospinning method are: the spinning voltage is between 20 kv and 40 kv, the receiving distance is between 10 cm and 20 cm, and the drum speed is between 90 r / min and 110 r / min.

[0040] In the PVDF dendritic nanofiber membrane prepared in S1, the diameter of the fiber trunk is between 100nm and 500nm, and the diameter of the branched fibers is between 5nm and 100nm.

[0041] The setting parameters of the hot pressing treatment in S2 are: pressure between 10MPa and 20MPa, temperature between 160°C and 180°C, and hot pressing time between 40min and 50min.

[0042] In S3, during the interfacial polymerization process using the interfacial polymerization method, the mass fraction of m-phenylenediamine is between 0.10 wt % and 0.20 wt %, and the mass fraction of tribenzoyl chloride is between 1 wt % and 3 wt %.

[0043] In S4, the polyamide film with the PVDF dendritic nanofiber membrane as the middle layer is placed in an oven for drying. The parameters set in the process are: the drying temperature is between 60° C. and 80° C., and the drying time is between 5 min and 15 min.

[0044] Embodiment 2

[0045] like Figure 1As shown, a PA membrane preparation process using a PVDF dendritic fiber membrane as a support layer includes the following steps: preparation of a PVDF dendritic nanofiber membrane and interfacial polymerization to form a polyamide film; the specific implementation method is as follows:

[0046] The raw materials for preparing a PA membrane with a PVDF dendritic fiber membrane as a support layer include but are not limited to: polyvinylidene fluoride (PVDF), tetrabutylammonium chloride (TBAC), PET non-woven fabric substrate, N,N-dimethylformamide (DMF), acetone, metaphenylenediamine (MPD), and tris-benzoyl chloride (TMC).

[0047] A. Preparation of PVDF dendritic nanofiber membrane:

[0048] A certain amount of PVDF and TBAC were dissolved in a mixed solution of DMF and acetone, and a spinning solution was obtained after uniform dissolution. The nanofiber membrane was prepared by high-voltage electrospinning technology, wherein the mass fraction of PVDF was 18wt%, and DMF:acetone was 3:1. During the spinning process, the spinning voltage was 3kV, the spinning distance was 20cm, and the spinning flow rate was 1mL / h. The dendritic nanostructures were as shown in FIG. Figure 2 As shown;

[0049] B. Configuration of MPD aqueous solution and TMC organic solution:

[0050] Weigh a certain amount of MPD, measure a corresponding volume of deionized water, dissolve MPD in water and stir to form a uniform solution; then weigh a certain amount of TMC and measure a corresponding amount of n-hexane in the same way, stir to form a uniform solution;

[0051] C. Formation of polyamide film:

[0052] The PVDF dendritic nanofiber membrane was fixed on a glass plate, and then the fixed membrane was immersed in a 2wt% MPD aqueous solution for 5 minutes, then taken out for surface drying, and then contacted with a 0.15wt% isopropanol solution for 2 minutes, and finally a polyamide TFC membrane was obtained by drying post-treatment.

[0053] Among them, what needs to be described in detail in the accompanying drawings is: Figure 2 The middle is the morphology of the PVDF dendritic nanofiber membrane in Example 1, from which a significant dendritic structure can be seen; Figure 3 This is a schematic diagram of interfacial polymerization in Example 1; Figure 4 This is a schematic diagram of the structure of a PA membrane using a PVDF dendritic fiber membrane as a support layer in Example 1; Figure 5 This is a morphology picture of the surface polyamide film of Example 1, from which an obvious ridge-valley structure can be seen.

[0054] Embodiment 3

[0055] In one embodiment, the preparation of the dendritic nanofibers in step S1 is specifically as follows: PVDF dendritic nanofibers are prepared by a high-voltage electrospinning method, with a spinning voltage of 30 kV, a receiving distance of 15 cm, and a drum speed of 100 r / min.

[0056] In one embodiment, the hot pressing post-treatment in step S2 is specifically as follows: placing the PVDF dendritic nanofiber membrane and the bottom PET nonwoven fabric into a hot press at a temperature of 170° C., a pressure of 15 MPa, and a pressing time of 45 min.

[0057] In one embodiment, the interfacial polymerization of step S3 is specifically as follows: the hot-pressed PVDF dendritic nanofiber membrane is fixed on a glass plate, the fixed membrane is immersed in a 2wt% MPD aqueous solution for 5 minutes, then taken out for surface drying, and then contacted with a 0.15wt% n-hexane solution for 2 minutes, and finally the PA TFC membrane is obtained by drying post-treatment.

[0058] In one embodiment, the oven parameters of step S4 are specifically set as follows: oven temperature is 70° C., and the time is 10 minutes.

[0059] In one embodiment, the PVDF dendritic nanofibers prepared in step S1 have a branch fiber diameter of 5-100 nm and a trunk fiber diameter of 100-500 nm.

[0060] In one embodiment, the solvent components in step S1 are N,N-dimethylformamide and acetone.

[0061] The second purpose of the present invention is to provide a new idea for the construction of a novel thin film composite membrane.

[0062] The third object of the present invention is to adapt the invented thin film composite membrane to sewage treatment and seawater desalination.

[0063] A fourth object of the present invention is to achieve high water flux while maintaining high rejection rate during operation of the thin film composite membrane of the present invention.

[0064] The fifth purpose of the present invention is the application of the thin film composite membrane of the present invention in industrial and chemical wastewater.

[0065] The sixth object of the present invention is that the thin film composite membrane of the present invention can be used in sewage treatment and seawater desalination.

[0066] It should be noted that the PVDF dendritic nanofiber membrane is a unique structure composed of ultrafine branched fibers and trunk fibers. Therefore, the PA membrane made with the PVDF dendritic fiber membrane as the support layer has a high specific surface area, porosity and interconnected porous structure. The ultrafine branched fibers can effectively reduce the pore size on the surface of the fiber membrane. In addition, the ultrafine branched fibers can form a direct water channel with the polyamide layer during interfacial polymerization. This unique structure can give it the potential for application in polyamide film composite membranes. The calculation formulas for the porosity, water flux and retention rate of the pore size of the dendritic membrane are as follows:

[0067] Porosity test: calculated by weight method, the formula is as follows:

[0068]

[0069] In the above formula, ε is the porosity of the membrane (%), m dry and m wet are the dry and wet masses of the membrane (g), ρ1 and ρ2 are the densities of the fiber membrane and ethanol (g / cm3).

[0070] Pore ​​size test: use PMI gas-liquid pore size analyzer to measure the membrane pore size.

[0071] Water flux test, the formula is as follows:

[0072]

[0073] In the above formula, J is the pure water flux, V is the volume, A is the membrane effective area, and t is the permeation time.

[0074] Retention rate test, the formula is as follows:

[0075]

[0076] In the above formula, R is the interception rate, C p and C f is the conductivity of the feed and permeate.

[0077] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as shown in the drawings and described above. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer, characterized in that: The steps include: S1: Preparation of PVDF dendritic nanofiber membrane by high-voltage electrospinning method; S2: hot pressing the PVDF dendritic nanofiber membrane prepared in S1; S3: fixing the PVDF dendritic nanofiber membrane obtained in S2 on a glass plate, using m-phenylenediamine and tribenzoyl chloride to form an ultra-thin polyamide film on the surface of the PVDF dendritic nanofiber membrane by an interfacial polymerization method, thereby forming a polyamide film composite membrane with the PVDF dendritic nanofiber membrane as an intermediate layer; S4: The polyamide film composite membrane with the PVDF dendritic nanofiber membrane as the middle layer obtained in S3 is rinsed with deionized water, and then placed in an oven for drying to obtain a PA membrane with the PVDF dendritic nanofiber membrane as the middle layer.

2. The method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer according to claim 1, characterized in that: The electrospinning parameters in the S1 medium and high voltage electrospinning method are: the spinning voltage is between 20 kv and 40 kv, the receiving distance is between 10 cm and 20 cm, and the drum speed is between 90 r / min and 110 r / min.

3. The method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer according to claim 1, characterized in that: In the PVDF dendritic nanofiber membrane prepared in S1, the diameter of the fiber trunk is between 100nm and 500nm, and the diameter of the branched fibers is between 5nm and 100nm.

4. The method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer according to claim 1, characterized in that: The setting parameters of the hot pressing treatment in S2 are: pressure between 10MPa and 20MPa, temperature between 160°C and 180°C, and hot pressing time between 40min and 50min.

5. The method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer according to claim 1, characterized in that: In S3, during the interfacial polymerization process using the interfacial polymerization method, the mass fraction of m-phenylenediamine is between 0.10 wt % and 0.20 wt %, and the mass fraction of tribenzoyl chloride is between 1 wt % and 3 wt %.

6. The method for preparing a PA membrane using a PVDF dendritic fiber membrane as a support layer according to claim 5, characterized in that: In S4, the polyamide film with the PVDF dendritic nanofiber membrane as the middle layer is placed in an oven for drying. The parameters set in the process are: the drying temperature is between 60° C. and 80° C., and the drying time is between 5 min and 15 min.

Citation Information

Patent Citations

  • KR20210116000A