Super-thick laminated coating battery insulation protective film
By using a laminated structure and thermal conductivity-enhancing materials in the battery insulation protective film, the problem of difficulty in balancing safety and heat dissipation performance with the thickness of the battery-specific protective film is solved, and better protection and thermal conductivity are achieved.
Patent Information
- Application Number
- CN202410978587.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The thickness of the existing battery-specific protective film cannot take into account the safety and heat dissipation performance of the battery. If it is too thin, it will easily cause a short circuit, while if it is too thick, it will affect the heat dissipation performance and cause damage to the battery safety performance.
A battery insulation protective film coated with an ultra-thick stack, including a first insulation film, a first adhesive, a second insulation film, a second adhesive and a third insulation film arranged in sequence from top to bottom, using polyimide material Acrylic resin is used as the base material, neodymium hexaboride powder with good thermal conductivity is added as the reinforcing material, and through activation treatment with an aldehyde coupling agent, a coated organic-based surface rich in triazine, Schiff base and other groups is prepared. Inorganic composite materials form a multi-layer protective film.
It improves the protective effect and thermal conductivity of the protective film, reduces the impact on the heat dissipation performance of the battery, enhances the adhesiveness, strength and high temperature resistance, and avoids the problem of battery overheating caused by being too thick.
Abstract
Description
Technical Field
[0001] The invention relates to the field of battery materials, and in particular to an ultra-thick laminated coated battery insulating protective film. Background Art
[0002] Power batteries are batteries used in new energy vehicles, and their stable operation as energy sources is critical. In the assembly and production process of new energy power lithium batteries, special insulating protective films are generally used to protect the outer shell of the power battery. The insulating protective film generally has three functions: first, to protect the battery, avoid short circuits between the positive and negative poles, and ensure the safe use of the battery; second, to insulate the electrolyte, which is one of the important components of the battery. The insulating protective film can prevent electrolyte leakage and protect the solid materials of the battery; third, to improve insulation. The insulating protective film can increase the insulation performance of the battery, ensure the stable performance of the battery, and extend the service life of the battery.
[0003] At present, the protective film for power batteries usually uses polymer film as the substrate, and the general total thickness is 60-100μm. The protective film for power batteries usually has good protection. Under normal circumstances, the thickness of the battery insulation protective film will directly affect the resistance of the battery, and then affect the performance of the battery. If it is too thin, it is easy to cause an internal short circuit in the battery, affecting the safety performance of the battery; if it is too thick, it will affect the heat dissipation performance of the battery, causing the battery to overheat, which will also affect the safety performance of the battery. Therefore, a battery insulation protective film is needed that can ensure safety and have a low impact on the heat dissipation performance of the battery. Summary of the invention
[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a battery insulation protection film with ultra-thick laminate coating.
[0005] The purpose of the present invention is achieved by adopting the following technical solutions:
[0006] An ultra-thick laminated battery insulating protective film comprises a first insulating film, a first adhesive, a second insulating film, a second adhesive and a third insulating film arranged in sequence from top to bottom; wherein the first insulating film, the second insulating film and the third insulating film are all made of polyimide material; the first adhesive and the second adhesive have the same composition, calculated by weight, and include:
[0007] 100 parts of acrylic resin, 11-24 parts of reinforcing material, 0.5-1.5 parts of dispersant, 0.2-0.8 parts of defoamer, 1-5 parts of curing agent and 40-60 parts of solvent.
[0008] Preferably, the grade of the polyimide material is any one of AURUM JCL3030, AURUM JCL6020 and AURUMJCN6230.
[0009] Preferably, the acrylic resin is a hydroxy acrylic resin, and the brand is a mixture of one or more of AC1018A, AC1010, AC3650, and AC3082.
[0010] Preferably, the dispersant is a mixture of one or more of octadecyltrimethylammonium chloride, sodium dodecylbenzenesulfonate, hexadecyltrimethylammonium chloride, and hexadecyltrimethylammonium p-toluenesulfonate.
[0011] Preferably, the defoaming agent is an organosilicon defoaming agent, and the brand is a mixture of one or more of AFE-0050, AFE-3168, and AFE-7610.
[0012] Preferably, the curing agent is an isocyanate curing agent, including toluene diisocyanate or hexamethylene diisocyanate.
[0013] Preferably, the solvent is ethyl acetate, ethylene glycol methyl ether or acetone.
[0014] Preferably, the method for preparing the reinforcing material comprises:
[0015] S1. Dispersing the neodymium hexaboride powder evenly in anhydrous ethanol, then adding 4-(triethoxysilyl)butyraldehyde, placing the mixture in a water bath, heating and stirring, and after the reaction is completed, cooling, centrifuging and drying are performed in sequence to obtain aldehyded neodymium hexaboride powder;
[0016] S2. Add aldehyded neodymium hexaboride powder and 2-amino-1,3,5-triazine into N-methylpyrrolidone respectively, stir them thoroughly, introduce nitrogen as a protective gas, heat and stir to react under the action of a catalyst, and successively cool, centrifuge and dry to obtain a reinforced material.
[0017] Preferably, in S1, the reaction treatment temperature is 65-85°C, the reaction treatment time is 6-12h, and the reaction stirring speed is 200-300r / min.
[0018] Preferably, in S1, the purity of the neodymium hexaboride powder is higher than 99%, and the particle size is 100±10 μm.
[0019] Preferably, in S1, the mass volume ratio of neodymium hexaboride powder, 4-(triethoxysilyl)butyraldehyde and anhydrous ethanol is 1 g:(0.23-0.46) g:(10-20) mL.
[0020] Preferably, in S2, the mass volume ratio of the formaldehyded neodymium hexaboride powder, 2-amino-1,3,5-triazine and N-methylpyrrolidone is 1 g:(0.32-0.64) g:(10-20) mL.
[0021] Preferably, in S2, the catalyst is anhydrous acetic acid, and the added amount is 3%-7% of the mass of 2-amino-1,3,5-triazine.
[0022] Preferably, in S2, the reaction temperature is 80-100°C, the reaction time is 4-8h, and the stirring speed is 200-300r / min.
[0023] Preferably, the first adhesive and the second adhesive are coated by slit coating.
[0024] Preferably, the thickness of the first insulating film, the second insulating film and the third insulating film is 20-40 μm, and the thickness of the first adhesive and the second adhesive is 15-25 μm.
[0025] Preferably, the preparation process of the first adhesive and the second adhesive includes: uniformly mixing the raw material components and stirring them uniformly in a stirring machine.
[0026] The beneficial effects of the present invention are:
[0027] 1. The present invention prepares an ultra-thick laminated battery insulation protective film, which uses a lamination method to compound the battery insulation film and adhesive to form a multi-layer protective film. The adhesive layer has a good heat dissipation effect. After the stacking of multiple layers of insulation films, compared with the traditional protective film, the protective film prepared by the present invention can maintain a certain thermal conductivity on the basis of increasing the thickness, which increases the protective effect of the protective film while minimizing the impact on the heat dissipation of the protective film.
[0028] 2. The adhesive added in the present invention is prepared by using acrylic resin as the base material and reinforcing material as the auxiliary material. The prepared adhesive not only has good viscosity and high temperature resistance, but also has good thermal conductivity, so that the heat dissipation effect of the protective film is improved, avoiding the influence of the heat dissipation performance of the battery due to excessive thickness.
[0029] 3. The reinforcing material in the adhesive of the present invention is a neodymium hexaboride powder with good thermal conductivity and poor electrical conductivity as a base material, which is activated by an aldehyde coupling agent to prepare aldehyde-modified neodymium hexaboride powder; then, an amine-aldehyde condensation reaction is carried out with 2-amino-1,3,5-triazine to prepare a coated organic-inorganic composite material with a surface rich in triazine, Schiff base and other groups, i.e., a reinforcing material. The reinforcing material is applied to the adhesive, and after testing, it is found that it not only has a good improvement in the heat dissipation of the resin, but also has a certain improvement in the adhesion, strength and high temperature resistance of the resin. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0031] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0032] The present invention will be further described below in conjunction with the following examples.
[0033] Example 1
[0034] An ultra-thick laminated battery insulation protective film includes a first insulating film, a first adhesive, a second insulating film, a second adhesive and a third insulating film arranged in sequence from top to bottom; wherein the first insulating film, the second insulating film and the third insulating film are all made of polyimide material; the grade of the polyimide material is AURUM JCL3030. The first adhesive and the second adhesive are coated by slit coating, the thickness of the first insulating film, the second insulating film and the third insulating film is 30 μm, and the thickness of the first adhesive and the second adhesive is 20 μm; after coating, it can be dried.
[0035] The first adhesive and the second adhesive have the same composition, calculated by weight, including:
[0036] 100 parts of acrylic resin, 18 parts of reinforcing material, 1 part of dispersant, 0.5 parts of defoamer, 3 parts of curing agent and 50 parts of solvent.
[0037] The acrylic resin is hydroxy acrylic resin, brand AC1018A. The dispersant is octadecyl trimethyl ammonium chloride. The defoamer is an organic silicon defoamer, brand AFE-0050. The curing agent is toluene diisocyanate. The solvent is ethyl acetate.
[0038] The preparation method of the reinforcement material comprises:
[0039] S1. Disperse neodymium hexaboride powder (purity higher than 99%, particle size of 100±10 μm) in anhydrous ethanol, then drop triethoxysilyl butyraldehyde, the mass volume ratio of neodymium hexaboride powder, 4-(triethoxysilyl) butyraldehyde and anhydrous ethanol is 1g:0.35g:15mL, place the mixed solution in a water bath, heat to 75°C and stir for 8h, the stirring speed is 250r / min, after the treatment is completed, naturally cool to room temperature, centrifuge to separate the solid, wash three times with water and vacuum dry at 60°C to obtain aldehyded neodymium hexaboride powder;
[0040] S2. Add formaldehyded neodymium hexaboride powder and 2-amino-1,3,5-triazine into N-methylpyrrolidone respectively. The mass volume ratio of formaldehyded neodymium hexaboride powder, 2-amino-1,3,5-triazine and N-methylpyrrolidone is 1g:0.48g:15mL. After fully stirring, introduce nitrogen as protective gas. Add anhydrous acetic acid dropwise as a catalyst in an amount of 5% of the mass of 2-amino-1,3,5-triazine. Stir the reaction in a 90°C water bath at a speed of 250r / min for 6h. After the reaction is completed, cool naturally to room temperature. Then separate the solid by centrifugation. Wash it three times with water and dry it in vacuum at 60°C to obtain a flame retardant material.
[0041] In the above, the preparation process of the first adhesive and the second adhesive includes: uniformly mixing the raw material components and stirring them uniformly in a stirring machine.
[0042] Example 2
[0043] An ultra-thick laminated battery insulating protective film includes a first insulating film, a first adhesive, a second insulating film, a second adhesive and a third insulating film arranged in sequence from top to bottom; wherein the first insulating film, the second insulating film and the third insulating film are all made of polyimide material; the grade of the polyimide material is AURUM JCL6020. The first adhesive and the second adhesive are coated by slit coating, the thickness of the first insulating film, the second insulating film and the third insulating film is 20 μm, and the thickness of the first adhesive and the second adhesive is 15 μm; after coating, it can be dried.
[0044] The first adhesive and the second adhesive have the same composition, calculated by weight, including:
[0045] 100 parts of acrylic resin, 11 parts of reinforcing material, 0.5 parts of dispersant, 0.2 parts of defoamer, 1 part of curing agent and 40 parts of solvent.
[0046] The acrylic resin is hydroxy acrylic resin, brand AC1010. The dispersant is sodium dodecylbenzene sulfonate. The defoamer is an organic silicon defoamer, brand AFE-3168. The curing agent is hexamethylene diisocyanate. The solvent is ethylene glycol methyl ether.
[0047] The preparation method of the reinforcement material comprises:
[0048] S1. Disperse neodymium hexaboride powder (purity higher than 99%, particle size of 100±10 μm) in anhydrous ethanol, then drop triethoxysilyl butyraldehyde, the mass volume ratio of neodymium hexaboride powder, 4-(triethoxysilyl) butyraldehyde and anhydrous ethanol is 1g:0.23g:10mL, place the mixed solution in a water bath, heat to 65°C and stir for 6h, the stirring speed is 200r / min, after the treatment is completed, naturally cool to room temperature, centrifuge to separate the solid, wash three times with water and vacuum dry at 60°C to obtain aldehyded neodymium hexaboride powder;
[0049] S2. Add formaldehyded neodymium hexaboride powder and 2-amino-1,3,5-triazine into N-methylpyrrolidone respectively. The mass volume ratio of formaldehyded neodymium hexaboride powder, 2-amino-1,3,5-triazine and N-methylpyrrolidone is 1g:0.32g:10mL. After fully stirring, introduce nitrogen as protective gas. Add anhydrous acetic acid dropwise as a catalyst in an amount of 3% of the mass of 2-amino-1,3,5-triazine. Stir the reaction in a water bath at 80°C for 4h at a stirring speed of 200r / min. After the reaction is completed, cool naturally to room temperature, then separate the solid by centrifugation, wash it three times with water, and dry it in a vacuum at 60°C to obtain a flame retardant material.
[0050] In the above, the preparation process of the first adhesive and the second adhesive includes: uniformly mixing the raw material components and stirring them uniformly in a stirring machine.
[0051] Example 3
[0052] An ultra-thick laminated battery insulating protective film includes a first insulating film, a first adhesive, a second insulating film, a second adhesive and a third insulating film arranged in sequence from top to bottom; wherein the first insulating film, the second insulating film and the third insulating film are all made of polyimide material; the grade of the polyimide material is AURUM JCN6230. The first adhesive and the second adhesive are coated by slit coating, the thickness of the first insulating film, the second insulating film and the third insulating film is 40 μm, and the thickness of the first adhesive and the second adhesive is 25 μm; after coating, it can be dried.
[0053] The first adhesive and the second adhesive have the same composition, calculated by weight, including:
[0054] 100 parts of acrylic resin, 24 parts of reinforcing material, 1.5 parts of dispersant, 0.8 parts of defoamer, 5 parts of curing agent and 60 parts of solvent.
[0055] The acrylic resin is hydroxy acrylic resin, brand AC3650. The dispersant is hexadecyl trimethyl ammonium chloride. The defoamer is an organic silicon defoamer, brand AFE-7610. The curing agent is an isocyanate curing agent, toluene diisocyanate. The solvent is acetone.
[0056] The preparation method of the reinforcement material comprises:
[0057] S1. Disperse neodymium hexaboride powder (purity higher than 99%, particle size of 100±10 μm) in anhydrous ethanol, then drop triethoxysilyl butyraldehyde, the mass volume ratio of neodymium hexaboride powder, 4-(triethoxysilyl) butyraldehyde and anhydrous ethanol is 1g:0.46g:20mL, place the mixed solution in a water bath, heat to 85°C and stir for 12h, the stirring speed is 300r / min, after the treatment is completed, naturally cool to room temperature, centrifuge to separate the solid, wash three times with water and vacuum dry at 60°C to obtain aldehyded neodymium hexaboride powder;
[0058] S2. Add formaldehyded neodymium hexaboride powder and 2-amino-1,3,5-triazine into N-methylpyrrolidone respectively. The mass volume ratio of formaldehyded neodymium hexaboride powder, 2-amino-1,3,5-triazine and N-methylpyrrolidone is 1g:0.64g:20mL. After fully stirring, introduce nitrogen as protective gas. Add anhydrous acetic acid dropwise as a catalyst in an amount of 7% of the mass of 2-amino-1,3,5-triazine. Stir the reaction in a water bath at 100°C for 8h at a stirring speed of 300r / min. After the reaction is completed, cool naturally to room temperature, then separate the solid by centrifugation, wash three times with water, and dry in vacuo at 60°C to obtain a flame retardant material.
[0059] In the above, the preparation process of the first adhesive and the second adhesive includes: uniformly mixing the raw material components and stirring them uniformly in a stirring machine.
[0060] Comparative Example 1
[0061] A battery insulating protective film, which is different from Example 1 only in that the components of the first adhesive and the second adhesive are different from those of Example 1. In this comparative example, the components of the first adhesive and the second adhesive are different from the fillers in Example 1. The adhesives are calculated by weight and include:
[0062] 100 parts of acrylic resin, 24 parts of neodymium hexaboride powder, 1.5 parts of dispersant, 0.8 parts of defoamer, 5 parts of curing agent and 60 parts of solvent.
[0063] The remaining ingredients are the same as those in Example 1.
[0064] Comparative Example 2
[0065] A battery insulating protective film, which differs from Example 1 only in that the components of the first adhesive and the second adhesive are different from those of Example 1. In this comparative example, the components of the first adhesive and the second adhesive are different from the fillers in Example 1. The components of the adhesives are calculated by weight and include:
[0066] 100 parts of acrylic resin, 24 parts of formaldehyded neodymium hexaboride powder (prepared in the same manner as in Example 1), 1.5 parts of dispersant, 0.8 parts of defoamer, 5 parts of curing agent and 60 parts of solvent.
[0067] The remaining ingredients are the same as those in Example 1.
[0068] Comparative Example 3
[0069] A battery insulating protective film, which differs from Example 1 only in that the components of the first adhesive and the second adhesive are different from those of Example 1. In this comparative example, the components of the first adhesive and the second adhesive are different from the fillers in Example 1. The components of the adhesives are calculated by weight and include:
[0070] 100 parts of acrylic resin, 24 parts of mixed filler (neodymium hexaboride powder and 2-amino-1,3,5-triazine mixed in a mass ratio of 1:0.48), 1.5 parts of dispersant, 0.8 parts of defoamer, 5 parts of curing agent and 60 parts of solvent.
[0071] The remaining ingredients are the same as those in Example 1.
[0072] Experimental testing
[0073] The adhesive prepared in Example 1 and Comparative Examples 1-3 was coated on a polyimide material of brand AURUM JCL3030. After being treated at 120° C. for 3 h, the properties of the adhesive were tested accordingly. The test items included bending strength, elongation at break, tensile strength under high temperature and high humidity, heat deformation temperature and thermal conductivity.
[0074] The testing standard for peel strength refers to GB / T 7122-1996, the testing standard for shear strength refers to GB / T 7124-2008, the testing standard for high temperature resistance refers to GB / T 16998-1997, and the testing standard for thermal conductivity refers to ASTM D5470.
[0075] The test results are shown in Table 1:
[0076] Table 1 Test results of different adhesives
[0077] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Peel strength (kN / m) 4.52 3.13 3.24 3.82 Shear strength(MPa) 37.9 32.5 33.7 35.4 High temperature resistance(℃) >200℃ 157 165 178 Thermal conductivity (W / (m·K)) 2.12 2.27 2.30 2.09
[0078] It can be seen from Table 1 that, compared with Comparative Examples 1-3, the adhesive prepared in Example 1 of the present invention has higher peel strength and shear strength, indicating that it has excellent adhesiveness and strength performance; in addition, it also has better high temperature resistance and thermal conductivity. This shows that the adhesive prepared in Example 1 of the present invention has excellent comprehensive performance and can be used in more severe environments.
[0079] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0080] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A battery insulation protective film with ultra-thick laminate coating, characterized in that: The invention comprises a first insulating film, a first adhesive, a second insulating film, a second adhesive and a third insulating film which are arranged in sequence from top to bottom; wherein the first insulating film, the second insulating film and the third insulating film are all made of polyimide material; the first adhesive and the second adhesive have the same composition, calculated by weight, and include: 100 parts of acrylic resin, 11-24 parts of reinforcing material, 0.5-1.5 parts of dispersant, 0.2-0.8 parts of defoamer, 1-5 parts of curing agent and 40-60 parts of solvent.
2. The battery insulation protective film with ultra-thick laminate coating according to claim 1, characterized in that: The grade of the polyimide material is any one of AURUM JCL3030, AURUM JCL6020 and AURUM JCN6230.
3. The battery insulation protective film with ultra-thick laminate coating according to claim 1, characterized in that: The acrylic resin is a hydroxy acrylic resin, and the brand is a mixture of one or more of AC1018A, AC1010, AC3650, and AC3082.
4. The battery insulation protective film with ultra-thick laminate coating according to claim 1, characterized in that: The dispersant is a mixture of one or more of octadecyltrimethylammonium chloride, sodium dodecylbenzenesulfonate, hexadecyltrimethylammonium chloride, and hexadecyltrimethylammonium p-toluenesulfonate.
5. The battery insulation protective film with ultra-thick laminate coating according to claim 1, characterized in that: The defoamer is an organosilicon defoamer, and the brand is a mixture of one or more of AFE-0050, AFE-3168, and AFE-7610.
6. The battery insulation protective film with ultra-thick laminate coating according to claim 1, characterized in that: The curing agent is an isocyanate curing agent, including toluene diisocyanate or hexamethylene diisocyanate; the solvent is ethyl acetate, ethylene glycol methyl ether or acetone.
7. The battery insulation protective film with ultra-thick laminate coating according to claim 1, characterized in that: The preparation method of the reinforcing material comprises: S1. Dispersing the neodymium hexaboride powder evenly in anhydrous ethanol, then adding 4-(triethoxysilyl)butyraldehyde, placing the mixture in a water bath, heating and stirring, and after the reaction is completed, cooling, centrifuging and drying are performed in sequence to obtain aldehyded neodymium hexaboride powder; S2. Add aldehyded neodymium hexaboride powder and 2-amino-1,3,5-triazine into N-methylpyrrolidone respectively, stir them thoroughly, introduce nitrogen as a protective gas, heat and stir to react under the action of a catalyst, and successively cool, centrifuge and dry to obtain a reinforced material.
8. The battery insulation protective film with ultra-thick laminate coating according to claim 7, characterized in that: In S1, the reaction temperature is 65-85°C, the reaction time is 6-12h, the stirring speed is 200-300r / min; the mass volume ratio of neodymium hexaboride powder, 4-(triethoxysilyl)butyraldehyde and anhydrous ethanol is 1g:(0.23-0.46)g:(10-20)mL.
9. The battery insulation protective film with ultra-thick laminate coating according to claim 7, characterized in that: In S2, the mass volume ratio of formaldehyded neodymium hexaboride powder, 2-amino-1,3,5-triazine and N-methylpyrrolidone is 1g:(0.32-0.64)g:(10-20)mL; the catalyst is anhydrous acetic acid, and the added amount is 3%-7% of the mass of 2-amino-1,3,5-triazine; the reaction temperature is 80-100°C, the reaction time is 4-8h, and the stirring speed is 200-300r / min.
10. The battery insulation protective film with ultra-thick laminate coating according to claim 1, characterized in that: The thickness of the first insulating film, the second insulating film and the third insulating film is 20-40 μm, and the thickness of the first adhesive and the second adhesive is 15-25 μm.
Citation Information
Patent Citations
High-performance electromagnetic shielding NdB6 / SiO2 multi-phase ceramic material and preparation method thereof
CN112573925A
Flexible lightweight solar cell panel assembly and preparation method thereof
CN114551624A
Heat-conducting insulating glue and preparation method thereof
CN117736679A
Power battery and module thereof
CN214625321U
Insulated wire
US20150206626A1
Cited By
Environment-friendly sole material with lightweight function and preparation method thereof
CN119931192A