Deep-texture decorative plate and preparation method thereof

By arranging cushions and decorative layers on building decorative panels and using modified materials, the flame retardant, impact resistance and water resistance properties of the panels are improved, the problems of flammability and insufficient functionality of existing panels are solved, and aesthetics are achieved and comprehensive improvement in performance.

CN118849599AActive Publication Date: 2024-10-29JIANGSU JIFU NEW MATERIAL

Patent Information

Application Number
CN202410867958.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-29
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

Most of the existing building decorative panels are combustible materials, which increase the fire load of the building. They are also insufficient in functionality and aesthetics, making it difficult to meet the comprehensive performance needs of modern buildings.

Method used

Adopting the preparation method of deep texture decorative boards, by setting cushion and decorative layers on the inner core board, using modified adhesives and modified coatings, combined with materials such as magnesium sulfate, magnesium oxide, fly ash and chitosan, to enhance the Flame retardant, impact resistance and water resistance properties of the board.

Benefits of technology

The deep-texture decorative board produced has good aesthetics, flame retardant performance, impact resistance and water resistance, and its comprehensive performance is significantly improved, reducing the amount of wood used, simplifying the preparation process, and improving market sales prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004920768750000111
    Figure BDA0004920768750000111
Patent Text Reader

Abstract

The invention discloses a deep-texture decorative plate and a preparation method thereof. The deep-texture decorative plate is composed of an inner core plate, a first cushion layer arranged on the upper surface of the inner core plate, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core plate and a second decorative layer arranged on the lower surface of the second cushion layer. The preparation method comprises the following steps: S1, respectively smearing an adhesive on the upper surface and the lower surface of the inner core plate, and carrying out plate pressing treatment on the first cushion layer and the second cushion layer; s2, adhesive is smeared on the upper surface and the lower surface of the material subjected to plate pressing in the step S1 correspondingly, and plate pressing treatment is conducted on the first decorative layer and the second decorative layer; s3, the outer surfaces of the first decorative layer and the second decorative layer are subjected to deburring treatment, then coated with modified paint and dried in the air, and the decorative film is obtained. The decorative plate is attractive in appearance, good in flame retardance, impact resistance and water resistance and good in comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plate preparation, and in particular relates to a deep-textured decorative plate and a preparation method thereof. Background Art

[0002] As an environmentally friendly material, wood has become one of the main materials in the world. However, with the advancement of technology and the improvement of people's use of wood, the amount of wood used is also increasing. The contradiction between the slow growth of trees and the increasing consumption of wood has put great pressure on forest resources. The shortage of resources requires people to save and use materials reasonably. In the new era, artificial boards have become one of the main building decoration materials.

[0003] New building materials are an important part of the building materials industry and an emerging industry in the building materials industry. With the gradual increase in the innovation of building materials and the efforts to save energy in buildings in my country, the improvement of building insulation, waterproofing, fire prevention, decoration and renovation standards, and the improvement of living conditions, the demand for new building materials will gradually increase. This demand makes building materials not only have good use functions, but also meet the pursuit of comfortable life. In addition, with the rapid development of the national economy and the substantial improvement of people's living standards, the industrial and civil building decoration and renovation industries have also developed rapidly, and people have put forward higher requirements for their living environment, especially in indoor decoration and renovation. People are not only satisfied with having a place to live, but more importantly, they hope that it has many functions such as safety and comfort. The proportion of the cost of decoration in the cost of the entire construction project is increasing. Unfortunately, a large number of decoration materials used in decoration and renovation operations, especially the building decoration and renovation panels currently used in the domestic market, are generally combustible or flammable materials. It is the large-scale use of these materials that increases the fire load of the building and buries hidden dangers for the indoor fire safety of the building.

[0004] In addition, with the improvement of people's living standards, various types of boards with good aesthetics and strong functionality have been developed and used, such as impact resistance, earthquake resistance, etc. In the prior art, for example, patent document CN101992653B provides a fireproof decorative board, which does not burn when exposed to fire, can self-extinguish after leaving the fire, and has good stability at high temperatures, and it only focuses on flame retardant properties; for example, patent document CN105291243A provides a production method for moisture-proof ceiling decorative boards, and the adhesive used is added with polyacrylate emulsion, polydimethylsiloxane and EVA latex on urea-formaldehyde resin, which improves the water resistance of urea-formaldehyde resin, and the prepared adhesive has good waterproof and moisture-proof properties, and the preparation process of the adhesive used is complicated.

[0005] Therefore, focusing on the research and development of a new decorative panel, the present invention hopes to provide a decorative panel with good comprehensive performance. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a deep-textured decorative board and a preparation method thereof. The resulting decorative board is beautiful and has good flame retardancy, impact resistance, water resistance and comprehensive performance.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] In a first aspect, the present invention provides a method for preparing a deep-textured decorative board, wherein the deep-textured decorative board comprises: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer;

[0009] The preparation method comprises the following steps:

[0010] S1. Apply adhesive to the upper and lower surfaces of the inner core plate respectively, and perform a pressing process on the first cushion layer and the second cushion layer;

[0011] S2, applying adhesive to the upper surface and the lower surface of the material after the pressing in step S1, and pressing the first decorative layer and the second decorative layer;

[0012] S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply modified coating, and dry them in the air.

[0013] In the above technical solution, the decorative board is a symmetrical structure, with an inner core board in the middle and cushion layers and decorative boards symmetrically arranged on both sides; the inner core board can be a common particle board, solid wood board, etc. As a protection, a film can also be attached to the surface of the obtained board to protect the board.

[0014] As a preferred embodiment of the technical solution of the present invention, the first decorative board and the second decorative board are both made of red cherry wood. The special deep texture of red cherry wood makes the made decorative boards beautiful and pretty.

[0015] As a preferred embodiment of the technical solution of the present invention, in step S1, the adhesive is a polyurethane adhesive, and the coating amount of the upper surface and the lower surface (i.e., the single-sided coating amount) is 100-150 g / m 2 ; The temperature of the pressing plate is room temperature, the pressure is 0.9~1.25MPa, and the time is 4~8h.

[0016] As a preferred embodiment of the technical solution of the present invention, in step S2, the adhesive is melamine-modified urea-formaldehyde resin; the coating amount of the upper surface and the lower surface (i.e., the single-sided coating amount) is 90-120 g / m 2 ; The temperature of the pressing plate is 90-110°C, the pressure is 0.8-1MPa, and the time is 30-60s.

[0017] As a preferred embodiment of the technical solution of the present invention, the preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps:

[0018] A1. Treat fly ash with a modifier, filter, wash and dry to obtain pre-modified fly ash;

[0019] A2, mixing magnesium sulfate, magnesium oxide and water to obtain a slurry, adding the modified fly ash obtained in step A1, mullite powder and chitosan to the slurry, and stirring again to obtain a secondary slurry;

[0020] A3. Extrude the obtained secondary slurry to form an embryo body, dry it and then cure it.

[0021] As a preferred embodiment of the technical solution of the present invention, in step A1, the modifier is obtained by mixing concentrated acid and hydrogen peroxide in a volume ratio of 1:1, and the mass concentration of hydrogen peroxide is 20-25%; the treatment time is 4-12 minutes, and the treatment temperature is room temperature.

[0022] As a preferred embodiment of the technical solution of the present invention, in step A2, the mass ratio of magnesium sulfate, magnesium oxide, water, modified fly ash, mullite and chitosan is: 1.5-4: 5.5-8: 10: 55-75: 4-8: 5-10.

[0023] As a preferred embodiment of the technical solution of the present invention, in step A3, the curing time is 2 to 4 days.

[0024] As a preferred embodiment of the technical solution of the present invention, in step S3, the coating amount of the modified coating is 0.05-0.2 mm; the preparation of the modified coating comprises the following steps:

[0025] B1. Mixing attapulgite with sodium hydroxide and treating the mixture at high temperature, grinding and sieving the mixture through a 50-150 mesh screen to obtain pre-modified attapulgite;

[0026] B2. Place silicon dioxide in a mixed solution of hydrogen peroxide and concentrated sulfuric acid and treat at room temperature for 1 to 6 minutes; after the treatment, filter, wash and dry to obtain pre-modified silicon dioxide;

[0027] B3. Add the pre-modified attapulgite obtained in step B1 to KH550, stir evenly, then add to phenolic resin, stir evenly again, add the pre-modified silica obtained in step B2, stir evenly, and obtain the modified coating.

[0028] As a preferred embodiment of the technical solution of the present invention, in step B1, the mass ratio of attapulgite to sodium hydroxide is 1:0.5-0.9; the high temperature treatment temperature is 780-800°C, and the treatment time is 0.5-4h;

[0029] In step B2, the volume ratio of hydrogen peroxide to concentrated sulfuric acid is 1:1, the mass concentration of hydrogen peroxide is 26-30%, and the amount ratio of silicon dioxide to the mixed solution is 1g:8-15mL;

[0030] In step B3, the mass ratio of pre-modified attapulgite, KH550, phenolic resin and pre-modified silica is 10-15:0.5-1:65:4-7.

[0031] In a second aspect, the present invention also intends to protect the deep-textured decorative board prepared by the above method.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention provides a method for preparing a deep-textured decorative board, which takes an inner core board as the main body, and presses a cushion layer and a decorative board on both sides. The use of the cushion layer reduces the amount of wood used and improves the performance of the decorative board.

[0034] (2) The present invention provides a method for preparing a deep-textured decorative board, which mainly uses a common adhesive and a conventional press plate processing process to prepare a decorative board, which is simple and easy to operate.

[0035] (3) The present invention provides a method for preparing a deep-textured decorative board. The cushion layer is prepared using magnesium sulfate and magnesium oxide as raw materials, which give the cushion layer excellent flame retardant properties. The cushion layer is prepared using inorganic materials as raw materials, which reduces the amount of wood used. At the same time, a large amount of fly ash and a small amount of chitosan and mullite are mixed into the raw materials. Fly ash is a type of by-product, and its utilization has great economic value and environmental significance. During use, the fly ash is treated with mixed acid to increase its specific surface area and reaction activity. The modified fly ash has a better effect in the cushion layer. The reason may be that after the reaction activity of the modified fly ash is improved, the small amount of silicate and acidic oxide it contains can react with magnesium sulfate and magnesium oxide accordingly, thereby improving the comprehensive performance of the material system. Of course, the modified fly ash also introduces hydroxyl groups, which is beneficial to the composite compatibility of fly ash and chitosan, reduces the agglomeration tendency of fly ash, and can also further improve the comprehensive performance of the cushion layer. It should be noted that the use of a small amount of chitosan can have an antibacterial effect on the one hand, and on the other hand, chitosan can also coordinate with magnesium ions to form a solid cross-linked structure, further improving the performance of the cushion layer; and the addition of mullite can be flame retardant on the one hand, and crack-resistant on the other hand, improving the performance of the cushion layer. In short, the use of the above substances cooperates with each other, so that the cushion layer has good impact resistance, good impact toughness, high bonding strength, and good comprehensive performance.

[0036] (3) The present invention provides a method for preparing a deep-textured decorative board. After the board is prepared, a specific coating is applied. The coating used uses phenolic resin as a film-forming agent and attapulgite and silicon dioxide as additives. During use, the attapulgite and silicon dioxide are treated accordingly to improve their agglomeration tendency and performance. Specifically, the attapulgite is treated with high-temperature alkali to enrich its pores and facilitate its subsequent composite with silicon dioxide after KH550 treatment. The silicon dioxide is treated with mixed acid like fly ash to increase its surface activity and introduce hydroxyl groups. The attapulgite modified with KH550 is rich in amino groups. The rich pores after high-temperature alkali treatment are conducive to forming a hydrogen bond system with silicon dioxide, forming a stable cross-linking system, and filling the dense phenolic resin film, thereby improving the coating effect and improving the mechanical properties and fire resistance of the board.

[0037] In short, the decorative board provided by the present invention is beautiful, has good comprehensive performance, and has good market sales prospects. DETAILED DESCRIPTION

[0038] Embodiments of the present invention are described in detail below. All embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0039] In the present invention, the brand of phenolic resin is F51; the mass fraction of concentrated sulfuric acid is 98%; the polyurethane adhesive can be selected from common products on the market, such as those sold by Shenzhen Yoshida Chemical Co., Ltd.; the melamine-modified urea-formaldehyde resin can be selected from common products on the market, such as the product sold by Gudeyuan Kente Technology (Beijing) Co., Ltd. with the brand GUUDPOLY MUF 207D; the particle size of silicon dioxide is about 50nm.

[0040] The inner core layer uses particle board as raw material; the first decorative board and the second decorative board are both red cherry wood; the thickness of the inner core board can be 3mm, the thickness of the decorative layer veneer is 0.2mm, the thickness of the cushion layer veneer is 0.8mm, and the total thickness of the decorative board is controlled at about 5mm; of course, it can also be produced in customized thickness according to customer needs.

[0041] In the present invention, the remaining unexplained parts are all conventional means known to those skilled in the art (such as coating methods, etc.); materials without source are all commercially available.

[0042] Example 1

[0043] A method for preparing a deep-textured decorative board, the deep-textured decorative board comprising: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer;

[0044] The preparation method comprises the following steps:

[0045] S1. Apply 125g / m2 of coating to the upper and lower surfaces of the inner core board. 2 Apply polyurethane adhesive respectively, and press the first cushion layer and the second cushion layer; the pressing process parameters are: room temperature, pressure 1.15MPa, time 5.5h;

[0046] S2: Apply 115 g / m2 of coating to the upper and lower surfaces of the material after the pressing plate in step S1. 2 The melamine-modified urea-formaldehyde resin is applied respectively, and the first decorative layer and the second decorative layer are subjected to a pressing process; the pressing process parameters are: temperature 105°C, pressure 0.95MPa, time 35s;

[0047] S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply 0.1 mm modified coating, and dry them.

[0048] The preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps:

[0049] A1. The fly ash was treated with a modifier (mixed with concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:1, with a hydrogen peroxide concentration of 20 wt%) for 5 min, and then filtered, washed, and dried to obtain pre-modified fly ash;

[0050] A2, mixing magnesium sulfate, magnesium oxide and water to obtain a slurry, adding the modified fly ash obtained in step A1, mullite powder and chitosan to the slurry, and stirring again to obtain a secondary slurry; wherein the mass ratio of magnesium sulfate, magnesium oxide, water, modified fly ash, mullite and chitosan is: 2.5:6:10:60:5:5.5;

[0051] A3. The obtained secondary slurry is extruded to form an embryo body (400×400 mm), which is then dried and cured for 3 days.

[0052] Wherein, the preparation of the modified coating comprises the following steps:

[0053] B1. Mix attapulgite and sodium hydroxide in a mass ratio of 1:0.6 and treat at 790°C for 1.5 hours. After treatment, grind and sieve 100 mesh to obtain pre-modified attapulgite;

[0054] B2. According to the dosage of 1g:10mL, silicon dioxide is placed in a mixed solution of hydrogen peroxide and concentrated sulfuric acid (volume ratio 1:1, hydrogen peroxide concentration 25wt%), and treated at room temperature for 3 minutes; after the treatment is completed, it is filtered, washed and dried to obtain pre-modified silicon dioxide;

[0055] B3. Add the pre-modified attapulgite obtained in step B1 to KH550, stir evenly, then add to phenolic resin, stir evenly again, add the pre-modified silica obtained in step B2, stir evenly, and obtain the modified coating; wherein the mass ratio of pre-modified attapulgite, KH550, phenolic resin, and pre-modified silica is 12:0.6:65:5.

[0056] Example 2

[0057] A method for preparing a deep-textured decorative board, the deep-textured decorative board comprising: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer;

[0058] The preparation method comprises the following steps:

[0059] S1. Apply 125g / m2 of coating to the upper and lower surfaces of the inner core board. 2 Apply polyurethane adhesive respectively, and press the first cushion layer and the second cushion layer; the pressing process parameters are: room temperature, pressure 1.15MPa, time 5.5h;

[0060] S2: Apply 115 g / m2 of coating to the upper and lower surfaces of the material after the pressing plate in step S1. 2 The melamine-modified urea-formaldehyde resin is applied respectively, and the first decorative layer and the second decorative layer are subjected to a pressing process; the pressing process parameters are: temperature 105°C, pressure 0.95MPa, time 35s;

[0061] S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply 0.1 mm modified coating, and dry them.

[0062] The preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps:

[0063] A1. Treat fly ash with a modifier (mixed with concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:1, with a hydrogen peroxide concentration of 20 wt%) for 4 min, and then filter, wash, and dry to obtain pre-modified fly ash;

[0064] A2, mixing magnesium sulfate, magnesium oxide and water to obtain a slurry, adding the modified fly ash obtained in step A1, mullite powder and chitosan to the slurry, and stirring again to obtain a secondary slurry; wherein the mass ratio of magnesium sulfate, magnesium oxide, water, modified fly ash, mullite and chitosan is: 2.5:6.5:10:65:4.5:6;

[0065] A3. The obtained secondary slurry is extruded to form an embryo body (400×400 mm), which is then dried and cured for 3 days.

[0066] Wherein, the preparation of the modified coating comprises the following steps:

[0067] B1. Mix attapulgite and sodium hydroxide in a mass ratio of 1:0.55 and treat at 795°C for 1 hour. After treatment, grind and sieve 100 mesh to obtain pre-modified attapulgite;

[0068] B2. According to the dosage of 1g:12mL, silicon dioxide is placed in a mixed solution of hydrogen peroxide and concentrated sulfuric acid (volume ratio 1:1, hydrogen peroxide concentration 25wt%), and treated at room temperature for 3 minutes; after the treatment is completed, it is filtered, washed and dried to obtain pre-modified silicon dioxide;

[0069] B3. Add the pre-modified attapulgite obtained in step B1 to KH550, stir evenly, then add to phenolic resin, stir evenly again, add the pre-modified silica obtained in step B2, stir evenly, and obtain the modified coating; wherein the mass ratio of pre-modified attapulgite, KH550, phenolic resin, and pre-modified silica is 12:0.65:65:5.5.

[0070] Example 3

[0071] A method for preparing a deep-textured decorative board, the deep-textured decorative board comprising: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer;

[0072] The preparation method comprises the following steps:

[0073] S1. Apply 125g / m2 of coating to the upper and lower surfaces of the inner core board. 2 Apply polyurethane adhesive respectively, and press the first cushion layer and the second cushion layer; the pressing process parameters are: room temperature, pressure 1.15MPa, time 5.5h;

[0074] S2: Apply 115 g / m2 of coating to the upper and lower surfaces of the material after the pressing plate in step S1. 2The melamine-modified urea-formaldehyde resin is applied respectively, and the first decorative layer and the second decorative layer are subjected to a pressing process; the pressing process parameters are: temperature 105°C, pressure 0.95MPa, time 35s;

[0075] S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply 0.1 mm modified coating, and dry them.

[0076] The preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps:

[0077] A1. Treat fly ash with a modifier (mixed with concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:1, with a hydrogen peroxide concentration of 20 wt%) for 4 min, and then filter, wash, and dry to obtain pre-modified fly ash;

[0078] A2, mixing magnesium sulfate, magnesium oxide and water to obtain a slurry, adding the modified fly ash obtained in step A1, mullite powder and chitosan to the slurry, and stirring again to obtain a secondary slurry; wherein the mass ratio of magnesium sulfate, magnesium oxide, water, modified fly ash, mullite and chitosan is: 2.5:5.5:10:65:5:5.5;

[0079] A3. The obtained secondary slurry is extruded to form an embryo body (400×400 mm), which is then dried and cured for 3 days.

[0080] Wherein, the preparation of the modified coating comprises the following steps:

[0081] B1. Mix attapulgite and sodium hydroxide in a mass ratio of 1:0.65 and treat at 790°C for 2 hours. After treatment, grind and sieve 100 mesh to obtain pre-modified attapulgite;

[0082] B2. According to the dosage of 1g:11mL, silicon dioxide is placed in a mixed solution of hydrogen peroxide and concentrated sulfuric acid (volume ratio 1:1, hydrogen peroxide concentration 25wt%), and treated at room temperature for 3 minutes; after the treatment is completed, it is filtered, washed and dried to obtain pre-modified silicon dioxide;

[0083] B3. Add the pre-modified attapulgite obtained in step B1 to KH550, stir evenly, then add to the phenolic resin, stir evenly again, add the pre-modified silica obtained in step B2, stir evenly, and obtain the modified coating; wherein the mass ratio of the pre-modified attapulgite, KH550, phenolic resin, and pre-modified silica is 11.5:0.55:65:6.

[0084] Comparative Example 1

[0085] Compared with Example 1, the preparation method of the first cushion layer and the second cushion layer in Comparative Example 1 omits step A1. Specifically, a preparation method of a deep-textured decorative board, the deep-textured decorative board comprises: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer;

[0086] The preparation method comprises the following steps:

[0087] S1. Apply 125g / m2 of coating to the upper and lower surfaces of the inner core board. 2 Apply polyurethane adhesive respectively, and press the first cushion layer and the second cushion layer; the pressing process parameters are: room temperature, pressure 1.15MPa, time 5.5h;

[0088] S2: Apply 115 g / m2 of coating to the upper and lower surfaces of the material after the pressing plate in step S1. 2 The melamine-modified urea-formaldehyde resin is applied respectively, and the first decorative layer and the second decorative layer are subjected to a pressing process; the pressing process parameters are: temperature 105°C, pressure 0.95MPa, time 35s;

[0089] S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply 0.1 mm modified coating, and dry them.

[0090] The preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps:

[0091] A1. Mix magnesium sulfate, magnesium oxide and water to obtain a slurry, add fly ash, mullite powder and chitosan to the slurry, and stir again to obtain a secondary slurry; wherein the mass ratio of magnesium sulfate, magnesium oxide, water, fly ash, mullite and chitosan is 2.5:6:10:60:5:5.5;

[0092] A2. The obtained secondary slurry is extruded to form an embryo body (400×400 mm), which is then dried and cured for 3 days.

[0093] Wherein, the preparation of the modified coating comprises the following steps:

[0094] B1. Mix attapulgite and sodium hydroxide in a mass ratio of 1:0.6 and treat at 790°C for 1.5 hours. After treatment, grind and sieve 100 mesh to obtain pre-modified attapulgite;

[0095] B2. According to the dosage of 1g:10mL, silicon dioxide is placed in a mixed solution of hydrogen peroxide and concentrated sulfuric acid (volume ratio 1:1, hydrogen peroxide concentration 25wt%), and treated at room temperature for 3 minutes; after the treatment is completed, it is filtered, washed and dried to obtain pre-modified silicon dioxide;

[0096] B3. Add the pre-modified attapulgite obtained in step B1 to KH550, stir evenly, then add to phenolic resin, stir evenly again, add the pre-modified silica obtained in step B2, stir evenly, and obtain the modified coating; wherein the mass ratio of pre-modified attapulgite, KH550, phenolic resin, and pre-modified silica is 12:0.6:65:5.

[0097] Comparative Example 2

[0098] Compared with Example 1, the preparation method of the first cushion layer and the second cushion layer in Comparative Example 2 omits the use of chitosan. Specifically, a preparation method of a deep texture decorative board, the deep texture decorative board is composed of: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer;

[0099] The preparation method comprises the following steps:

[0100] S1. Apply 125g / m2 of coating to the upper and lower surfaces of the inner core board. 2 Apply polyurethane adhesive respectively, and press the first cushion layer and the second cushion layer; the pressing process parameters are: room temperature, pressure 1.15MPa, time 5.5h;

[0101] S2: Apply 115 g / m2 of coating to the upper and lower surfaces of the material after the pressing plate in step S1. 2 The melamine-modified urea-formaldehyde resin is applied respectively, and the first decorative layer and the second decorative layer are subjected to a pressing process; the pressing process parameters are: temperature 105°C, pressure 0.95MPa, time 35s;

[0102] S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply 0.1 mm modified coating, and dry them.

[0103] The preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps:

[0104] A1. The fly ash was treated with a modifier (mixed with concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:1, with a hydrogen peroxide concentration of 20 wt%) for 5 min, and then filtered, washed, and dried to obtain pre-modified fly ash;

[0105] A2, mixing magnesium sulfate, magnesium oxide and water to obtain a slurry, adding the modified fly ash obtained in step A1 and mullite powder to the slurry, and stirring again to obtain a secondary slurry; wherein the mass ratio of magnesium sulfate, magnesium oxide, water, modified fly ash and mullite is: 2.5:6:10:60:5;

[0106] A3. The obtained secondary slurry is extruded to form an embryo body (400×400 mm), which is then dried and cured for 3 days.

[0107] Wherein, the preparation of the modified coating comprises the following steps:

[0108] B1. Mix attapulgite and sodium hydroxide in a mass ratio of 1:0.6 and treat at 790°C for 1.5 hours. After treatment, grind and sieve 100 mesh to obtain pre-modified attapulgite;

[0109] B2. According to the dosage of 1g:10mL, silicon dioxide is placed in a mixed solution of hydrogen peroxide and concentrated sulfuric acid (volume ratio 1:1, hydrogen peroxide concentration 25wt%), and treated at room temperature for 3 minutes; after the treatment is completed, it is filtered, washed and dried to obtain pre-modified silicon dioxide;

[0110] B3. Add the pre-modified attapulgite obtained in step B1 to KH550, stir evenly, then add to phenolic resin, stir evenly again, add the pre-modified silica obtained in step B2, stir evenly, and obtain the modified coating; wherein the mass ratio of pre-modified attapulgite, KH550, phenolic resin, and pre-modified silica is 12:0.6:65:5.

[0111] Comparative Example 3

[0112] Compared with Example 1, Comparative Example 3 omits the modification of attapulgite in the modified coating, that is, attapulgite is directly used without any modification; specifically, a method for preparing a deep-textured decorative board, the deep-textured decorative board comprises: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer;

[0113] The preparation method comprises the following steps:

[0114] S1. Apply 125g / m2 of coating to the upper and lower surfaces of the inner core board. 2 Apply polyurethane adhesive respectively, and press the first cushion layer and the second cushion layer; the pressing process parameters are: room temperature, pressure 1.15MPa, time 5.5h;

[0115] S2: Apply 115 g / m2 of coating to the upper and lower surfaces of the material after the pressing plate in step S1. 2 The melamine-modified urea-formaldehyde resin is applied respectively, and the first decorative layer and the second decorative layer are subjected to a pressing process; the pressing process parameters are: temperature 105°C, pressure 0.95MPa, time 35s;

[0116] S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply 0.1 mm modified coating, and dry them.

[0117] The preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps:

[0118] A1. The fly ash was treated with a modifier (mixed with concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:1, with a hydrogen peroxide concentration of 20 wt%) for 5 min, and then filtered, washed, and dried to obtain pre-modified fly ash;

[0119] A2, mixing magnesium sulfate, magnesium oxide and water to obtain a slurry, adding the modified fly ash obtained in step A1, mullite powder and chitosan to the slurry, and stirring again to obtain a secondary slurry; wherein the mass ratio of magnesium sulfate, magnesium oxide, water, modified fly ash, mullite and chitosan is: 2.5:6:10:60:5:5.5;

[0120] A3. The obtained secondary slurry is extruded to form an embryo body (400×400 mm), which is then dried and cured for 3 days.

[0121] Wherein, the preparation of the modified coating comprises the following steps:

[0122] B1. According to the dosage of 1g:10mL, silicon dioxide is placed in a mixed solution of hydrogen peroxide and concentrated sulfuric acid (volume ratio 1:1, hydrogen peroxide concentration 25wt%), and treated at room temperature for 3 minutes; after the treatment is completed, it is filtered, washed and dried to obtain pre-modified silicon dioxide;

[0123] B2. Add attapulgite to KH550, stir evenly, then add to phenolic resin, stir evenly again, add the pre-modified silica obtained in step B1, stir evenly, and obtain the modified coating; wherein the mass ratio of attapulgite, KH550, phenolic resin, and pre-modified silica is 12:0.6:65:5.

[0124] Comparative Example 4

[0125] Compared with Example 1, Comparative Example 4 omits the modification of silicon dioxide, that is, directly uses silicon dioxide. Specifically: a method for preparing a deep-textured decorative board, the deep-textured decorative board comprises: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer;

[0126] The preparation method comprises the following steps:

[0127] S1. Apply 125g / m2 of coating to the upper and lower surfaces of the inner core board. 2 Apply polyurethane adhesive respectively, and press the first cushion layer and the second cushion layer; the pressing process parameters are: room temperature, pressure 1.15MPa, time 5.5h;

[0128] S2: Apply 115 g / m2 of coating to the upper and lower surfaces of the material after the pressing plate in step S1. 2 The melamine-modified urea-formaldehyde resin is applied respectively, and the first decorative layer and the second decorative layer are subjected to a pressing process; the pressing process parameters are: temperature 105°C, pressure 0.95MPa, time 35s;

[0129] S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply 0.1 mm modified coating, and dry them.

[0130] The preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps:

[0131] A1. The fly ash was treated with a modifier (mixed with concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:1, with a hydrogen peroxide concentration of 20 wt%) for 5 min, and then filtered, washed, and dried to obtain pre-modified fly ash;

[0132] A2, mixing magnesium sulfate, magnesium oxide and water to obtain a slurry, adding the modified fly ash obtained in step A1, mullite powder and chitosan to the slurry, and stirring again to obtain a secondary slurry; wherein the mass ratio of magnesium sulfate, magnesium oxide, water, modified fly ash, mullite and chitosan is: 2.5:6:10:60:5:5.5;

[0133] A3. The obtained secondary slurry is extruded to form an embryo body (400×400 mm), which is then dried and cured for 3 days.

[0134] Wherein, the preparation of the modified coating comprises the following steps:

[0135] B1. Mix attapulgite and sodium hydroxide in a mass ratio of 1:0.6 and treat at 790°C for 1.5 hours. After treatment, grind and sieve 100 mesh to obtain pre-modified attapulgite;

[0136] B2. Add the pre-modified attapulgite obtained in step B1 to KH550, stir evenly, then add to phenolic resin, stir evenly again, add silicon dioxide, stir evenly, and obtain the modified coating; wherein the mass ratio of pre-modified attapulgite, KH550, phenolic resin, and silicon dioxide is 12:0.6:65:5.

[0137] First, the intermediate plate products obtained after the treatment in step S1 in Example 1 and Comparative Examples 1-2 are subjected to performance tests;

[0138] 1) Impact toughness performance test: refer to GB / T 17657-2022 for room temperature impact toughness and low temperature impact toughness performance tests.

[0139] 2) Screw holding force test: refer to GB / T 17657-2022 to test the front screw holding force and side screw holding force.

[0140] 3) Elastic modulus test: refer to GB / T 17657-2022.

[0141] 4) Bonding strength test: refer to GB / T 17657-2022.

[0142] 5) Impact resistance test: refer to GB / T 17657-2022.

[0143] Table 1 Middle board performance test

[0144]

[0145] Next, the deep texture decorative panels prepared in Example 1 and Comparative Examples 2 to 4 were subjected to performance tests, and the specific methods are as follows:

[0146] 1) Flame retardancy test: Flame retardancy grade classification is carried out according to GB8624-2012 and testing is carried out according to GB / T 8626-2007; oxygen index test is carried out according to GB / T 2406-2009.

[0147] 2) Immersion peeling test: refer to GB / T17657-2022, and the board size is cut to 75×75mm.

[0148] 3) Wear resistance test: refer to method 3 in GB / T17657-2022, rotate 200 times, weigh the plate before and after grinding, calculate the difference, and get the loss.

[0149] Table 2 Decorative board performance test

[0150] Flame retardant grade Oxygen Index Dip stripping Loss / g Example 1 Level A 36 qualified 0.201 Comparative Example 3 Level A 32 qualified 0.254 Comparative Example 4 Level A 28 Failure 0.386

[0151] It can be seen from Table 1 that the cushion layer prepared in the present application has good impact resistance, impact toughness, elastic modulus and bonding strength, which ensures the performance of the prepared decorative board; from the test results in Table 2, it can be seen that the decorative board prepared in the present application has good fire resistance, low loss and excellent comprehensive performance.

[0152] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a deep texture decorative board, characterized in that: The deep texture decorative board is composed of: an inner core board, a first cushion layer arranged on the upper surface of the inner core board, a first decorative layer arranged on the upper surface of the first cushion layer, a second cushion layer arranged on the lower surface of the inner core board, and a second decorative layer arranged on the lower surface of the second cushion layer; The preparation method comprises the following steps: S1. Apply adhesive to the upper and lower surfaces of the inner core plate respectively, and perform a pressing process on the first cushion layer and the second cushion layer; S2, applying adhesive to the upper surface and the lower surface of the material after the pressing in step S1, and pressing the first decorative layer and the second decorative layer; S3, after deburring the outer surfaces of the first decorative layer and the second decorative layer, apply modified coating, and dry them in the air.

2. The method for preparing a deep texture decorative board according to claim 1, characterized in that: The first decorative panel and the second decorative panel are both made of red cherry wood.

3. The method for preparing a deep texture decorative board according to claim 1, characterized in that: In step S1, the adhesive is a polyurethane adhesive, and the coating amount on the upper surface and the lower surface is 100-150 g / m 2 ; The temperature of the pressing plate is room temperature, the pressure is 0.9~1.25MPa, and the time is 4~8h.

4. The method for preparing a deep texture decorative board according to claim 1, characterized in that: In step S2, the adhesive is melamine-modified urea-formaldehyde resin; the coating amount of the upper surface and the lower surface is 90-120 g / m 2 ; The temperature of the pressing plate is 90-110°C, the pressure is 0.8-1MPa, and the time is 30-60s.

5. The method for preparing a deep texture decorative board according to claim 1, characterized in that: The preparation methods of the first cushion layer and the second cushion layer are the same, comprising the following steps: A1. Treat fly ash with a modifier, filter, wash and dry to obtain pre-modified fly ash; A2, mixing magnesium sulfate, magnesium oxide and water to obtain a slurry, adding the modified fly ash obtained in step A1, mullite powder and chitosan to the slurry, and stirring again to obtain a secondary slurry; A3. The obtained secondary slurry is squeezed to form an embryo body, which is then dried and cured to obtain an embryo body.

6. The method for preparing a deep texture decorative board according to claim 5, characterized in that: In step A1, the modifier is obtained by mixing concentrated acid and hydrogen peroxide in a volume ratio of 1:1, and the mass concentration of hydrogen peroxide is 20-25%; the treatment time is 4-12 minutes, and the treatment temperature is room temperature.

7. The method for preparing a deep texture decorative board according to claim 5, characterized in that: In step A2, the mass ratio of magnesium sulfate, magnesium oxide, water, modified fly ash, mullite and chitosan is: 1.5-4: 5.5-8: 10: 55-75: 4-8: 5-10.

8. The method for preparing a deep texture decorative board according to claim 1, characterized in that: In step S3, the coating amount of the modified coating is 0.05-0.2 mm; the preparation of the modified coating comprises the following steps: B1. Mixing attapulgite with sodium hydroxide and treating the mixture at high temperature, grinding and sieving the mixture through a 50-150 mesh screen to obtain pre-modified attapulgite; B2. Place silicon dioxide in a mixed solution of hydrogen peroxide and concentrated sulfuric acid and treat at room temperature for 1 to 6 minutes; after the treatment, filter, wash and dry to obtain pre-modified silicon dioxide; B3. Add the pre-modified attapulgite obtained in step B1 to KH550, stir evenly, then add to phenolic resin, stir evenly again, add the pre-modified silica obtained in step B2, stir evenly, and obtain the modified coating.

9. The method for preparing a deep texture decorative board according to claim 8, characterized in that: In step B1, the mass ratio of attapulgite to sodium hydroxide is 1:0.5-0.9; the high temperature treatment temperature is 780-800°C, and the treatment time is 0.5-4h; In step B2, the volume ratio of hydrogen peroxide to concentrated sulfuric acid is 1:1, the mass concentration of hydrogen peroxide is 26-30%, and the amount ratio of silicon dioxide to the mixed solution is 1g:8-15mL; In step B3, the mass ratio of pre-modified attapulgite, KH550, phenolic resin and pre-modified silica is 10-15:0.5-1:65:4-7.

10. A deep texture decorative board prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Production formula of iron and magnesium composite modified fly ash

    CN102838305A

  • Alcohol-based foundry coating of light burned dolomite and fabrication method thereof

    CN104014721A

  • Anti-corrosion and flame retardant coating

    CN104194572A

  • Corrosion-resistant raw lacquer coating as well as preparation method and application thereof

    CN115851129A

  • Liquid fertilizer as well as preparation method and application thereof

    CN116143555A

Cited By

  • TPU (thermoplastic polyurethane) material and preparation process thereof

    CN119371810A

  • Iodine-resistant packaging material and preparation method thereof

    CN119526874A

  • Iodine-blocking packaging material and preparation method thereof

    CN119526874B