Method and device for preparing high-yield and high-purity single-walled carbon nanotubes

Through improved preparation methods and devices, using technologies such as micro-positive pressure and carbon monoxide calcination, the problem of insufficient quality and purity of single-walled carbon nanotubes in traditional methods has been solved, and high-yield and high-purity single-walled carbon nanotubes have been prepared.

CN118851160APending Publication Date: 2024-10-29厦门华碳科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410842459.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing traditional methods in single-walled carbon nanotube synthesis have poor quality and poor removal of coarse iron oxide, resulting in insufficient yield and purity.

Method used

Using improved preparation methods and devices, including mixing liquid carbon sources, metal compounds, cocatalysts and modifiers in a certain proportion, processing in a high-temperature furnace and depositing in a slightly positive pressure environment, followed by carbon monoxide calcination and pickling to remove impurities, Improve the exhaust pipe structure to increase the furnace pressure and promote the rapid deposition and purification of single-walled carbon nanotubes.

Benefits of technology

It achieves the preparation of high-yield, high-purity single-walled carbon nanotubes, significantly improves the graphitization degree and impurity removal efficiency of the product, and ensures the high-quality production of single-walled carbon nanotubes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851160A_ABST
    Figure CN118851160A_ABST
Patent Text Reader

Abstract

According to the preparation method and device of the high-yield and high-purity single-walled carbon nanotube, heated gas is introduced from the outside of a sleeve quartz tube, so that uniform heating of the gas and stability of a system are facilitated; reducing gas and protective gas are heated in a gas mixing tank before being fed into a high-temperature furnace tube, micro-positive pressure is provided for a preparation system, and rapid growth and deposition of the single-walled carbon nanotubes are improved; and the high-temperature heating of the gas can enable the single-walled carbon nanotube to enter the system to reach a proper growth temperature. Meanwhile, the caliber of the tail gas pipe is reduced, so that the pressure in the furnace pipe is increased, and the deposition process of the single-walled carbon nanotubes in a system is rapidly promoted; the regulation and control of the micro-positive pressure system are tested and monitored through a pressure gauge, so that the growth conditions of high-quality and high-yield single-walled carbon nanotubes are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of single-walled carbon nanotube materials, and in particular to a method and device for preparing single-walled carbon nanotubes with high yield and purity. Background Art

[0002] The characteristics of single-walled carbon nanotubes include light weight, ability to withstand high pressure and temperature, strong wear resistance, high aspect ratio, high modulus and strength, etc. Therefore, single-walled carbon nanotubes can be used to improve metal materials and polymer materials to prepare high-strength, lightning-resistant, invisible, and low-temperature and anti-icing materials. In addition, due to the unique physical properties of single-walled carbon nanotubes, they have a wide range of applications in chip technology, lithium-ion batteries, aerospace materials, rubber, plastics and other fields.

[0003] Chemical vapor deposition is one of the common methods for synthesizing single-walled carbon nanotubes. This method is to introduce carbon source gas and catalyst into a vertical tube furnace at high temperature for reaction. The vertical tube furnace provides a suitable reaction environment, which can maintain a suitable temperature and atmosphere to promote the decomposition of carbon source gas and the growth of single-walled carbon nanotubes. Therefore, chemical vapor deposition and vertical tube furnace are inseparable. They depend on each other and interact with each other to achieve efficient preparation of single-walled carbon nanotubes.

[0004] However, the existing conventional machine directly introduces gas into a vertical tube furnace to participate in the reaction, resulting in poor quality of single-walled carbon nanotube synthesis, and poor removal effect of partial iron oxide caused by direct acid washing of the synthesized single-walled carbon nanotube coarse powder. Summary of the invention

[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide a method and device for preparing single-walled carbon nanotubes with high yield and high purity.

[0006] The first aspect of the present application provides a method for preparing single-walled carbon nanotubes with high yield and high purity, comprising the following steps:

[0007] (1) preparing a dispersion liquid with a liquid carbon source, a metal compound, a co-catalyst and a modifier in a certain proportion;

[0008] (2) The reducing gas methane and the protective gas enter the mixing tank together at a certain flow ratio for heating and mixing, and are introduced into the furnace tube of the high-temperature furnace after stabilization;

[0009] (3) The dispersion is introduced into a high temperature furnace at a certain injection speed, and the crude product is collected every 20-40 minutes;

[0010] (4) The crude product is calcined for a period of time to remove amorphous carbon on the surface; then, concentrated acid is used for stirring at a certain temperature for a period of time to remove metal impurities in the crude product.

[0011] In any embodiment, the liquid carbon source is one or more of toluene and benzyl alcohol; the metal compound is one or more of cobaltocene, ferrocene, and nickelocene; the co-catalyst is one or more of thiophenol and selenophene; the modifier is one or more of ethanol and ethylene glycol; the usage ratio of the metal compound, liquid carbon source, co-catalyst and modifier is 2-6g:60-180mL:2-6mL:20-25mL.

[0012] In any embodiment, the reducing gas is methane, the shielding gas is nitrogen, and the ratio of the reducing gas to the shielding gas is 5000-7000 sccm:2500 sccm.

[0013] In any embodiment, the injection speed of the dispersion in step (3) is 180-210 μL / min; the furnace tube temperature of the high-temperature furnace is 1150-1200°C.

[0014] In any embodiment, in step (4), the crude product is calcined in air at 1000-1400° C.; the air oxidation time of the crude product is 1-2 h.

[0015] In any embodiment, after removing amorphous carbon in step (4), calcination is continued by introducing carbon monoxide.

[0016] In any embodiment, the carbon monoxide is introduced at 200-400 sccm and calcined for 1-2 hours at a calcination temperature of 1000-1400°C.

[0017] In any embodiment, the concentrated acid is concentrated hydrochloric acid or concentrated sulfuric acid; the stirring temperature is 30-40° C., and the stirring time is 6-8 h.

[0018] The second aspect of the present application also provides a device for preparing single-walled carbon nanotubes with high yield and high purity, comprising a gas cylinder, a gas mixing tank and a vertical tubular furnace connected in sequence, and an injector connected to the vertical tubular furnace, wherein the outlets of the gas mixing tank and the injector are both connected to the inlet of the vertical tubular furnace, and the vertical tubular furnace is provided with a tail gas pipe.

[0019] In any embodiment, the heating temperature of the gas mixing tank is 500-800° C.; the diameter of the tail gas pipe is 25-35 mm.

[0020] Beneficial effects of the present application: The device of the present invention, by modifying the traditional machine, adds a step of heating the gas to 800°C before the gas is fed into the mixing tank, aiming to make the system inside the furnace tube in a state of slightly positive pressure (0.3-0.5mPa), and to make the coarse tail gas pipe thinner to slow down the exhaust gas emission rate, increase the pressure inside the furnace body, and promote the rapid deposition of single-walled carbon nanotubes; and improve the adverse consequences of partial incomplete removal of iron oxide caused by direct acid washing of single-walled carbon nanotube coarse powder in the traditional scheme, by introducing carbon monoxide during the heating process to reduce iron oxide to iron, and then acid washing with sulfuric acid or hydrochloric acid, which makes it easier to remove iron impurities. The present application realizes the large-scale synthesis of high-quality single-walled carbon nanotubes. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic structural diagram of a device for preparing single-walled carbon nanotubes with high yield and purity according to the present application;

[0022] Figure 2 This is a schematic diagram of the sleeve structure of a high-yield and high-purity single-walled carbon nanotube preparation device of the present application;

[0023] Figure 3 This is a method for preparing single-walled carbon nanotubes with high yield and purity in this application. Example 1 is a scanning electron microscope image of the purified product;

[0024] Figure 4 A method for preparing single-walled carbon nanotubes with high yield and purity is provided in this application. Example 1 Raman image of the purified product;

[0025] Figure 5 This is a scanning electron microscope image of the purified product of Example 2 of a method for preparing single-walled carbon nanotubes with high yield and purity of the present application;

[0026] Figure 6 This is a method for preparing single-walled carbon nanotubes with high yield and high purity in this application. Example 2 Raman map of the purified product;

[0027] Figure 7 This is a scanning electron microscope image of the purified product of Example 3 of a method for preparing single-walled carbon nanotubes with high yield and purity of the present application;

[0028] Figure 8 This is a method for preparing single-walled carbon nanotubes with high yield and high purity in this application. Example 3 Raman image of the purified product;

[0029] Fig. 9 This is a scanning electron microscope image of the purified product of Comparative Example 1;

[0030] Fig.10 This is the Raman image of the purified product in Comparative Example 1;

[0031] Fig.11 This is a scanning electron micrograph of the purified product of Comparative Example 2;

[0032] Fig.12 This is the Raman image of the purified product in Comparative Example 2.

[0033] Description of reference numerals:

[0034] Gas cylinder 1; gas mixing tank 2; vertical tube furnace 3; injector 4; tail gas pipe 31; casing 5; air inlet pipe 51; liquid inlet pipe 52. DETAILED DESCRIPTION

[0035] Hereinafter, an embodiment of a method and apparatus for preparing single-walled carbon nanotubes with high yield and high purity of the present application will be specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0036] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0037] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0038] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0039] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0040] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0041] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0042] A method for preparing single-walled carbon nanotubes with high yield and purity comprises the following steps:

[0043] (1) A liquid carbon source, a metal compound, a co-catalyst and a modifier are prepared into a dispersion according to a certain ratio; the liquid carbon source is one or more of toluene and benzyl alcohol; the metal compound is one or more of cobaltocene, ferrocene and nickelocene; the co-catalyst is one or more of thiophenol and selenophene; the modifier is one or more of ethanol and ethylene glycol; the amount ratio of the metal compound, the liquid carbon source, the co-catalyst and the modifier is 2-6g: 60-180mL: 2-6mL: 20-25mL.

[0044] (2) The reducing gas methane and the protective gas enter the mixing tank together at a certain flow ratio for heating and mixing, and are introduced into the furnace tube of the high-temperature furnace after stabilization; the reducing gas is methane, the protective gas is nitrogen, and the ratio of the reducing gas to the protective gas is 5000-7000sccm:2500sccm.

[0045] (3) The dispersion is introduced into a high-temperature furnace at a certain injection speed, and the crude product is collected once every 20-40 minutes; the injection speed of the dispersion is 180-210 μL / min; and the furnace tube temperature of the high-temperature furnace is 1150-1200°C.

[0046] (4) The crude product is continuously calcined for a period of time to remove amorphous carbon on the surface; then, concentrated acid is used to stir for a period of time at a certain temperature to remove metal impurities in the crude product. The crude product is air calcined at 1000-1400°C; the air oxidation time of the crude product is 1-2h; after removing amorphous carbon in step (4), calcination is continued at 1000-1400°C for 1-2h while introducing 200-400sccm carbon monoxide; the concentrated acid is concentrated hydrochloric acid or concentrated sulfuric acid; the stirring temperature is 30-40°C and the time is 6-8h.

[0047] A high-yield and high-purity single-walled carbon nanotube preparation device comprises a gas cylinder 1, a gas mixing tank 2 and a vertical tube furnace 3 connected in sequence, and an injector 4 connected to the vertical tube furnace 3, wherein the outlets of the gas mixing tank 2 and the injector 4 are both connected to the inlet of the vertical tube furnace 3, and the vertical tube furnace 3 is provided with a tail gas pipe 31. The heating temperature of the gas mixing tank 2 is 500-800°C; the diameter of the tail gas pipe 31 is 25-35mm.

[0048] In the preparation of high-yield and high-purity single-walled carbon nanotubes, micro-positive pressure regulation is used to prepare high-yield and high-purity single-walled carbon nanotubes, which is mainly divided into three steps: preparing dispersion liquid, synthesizing crude products and purification treatment.

[0049] Preparing a dispersion: mixing a liquid carbon source, a metal compound, a sulfur source and an etchant together to prepare a dispersion.

[0050] Synthesizing crude product: Inject the dispersion through the top of the high-temperature furnace, introduce reducing gas and protective gas at the same time, and use the floating catalytic method to synthesize single-walled carbon nanotubes; during this process, the crude product will be deposited in the lower part of the high-temperature furnace and the collection tank.

[0051] Purification treatment: Take out the crude product synthesized above and purify it. Use methods such as high-temperature calcination with CO to remove amorphous carbon and increase the degree of graphitization; at the same time, strong acid stirring can be used to remove metal impurities and other impurities to obtain purer and higher-quality single-walled carbon nanotubes.

[0052] The specific process is as follows:

[0053] (1) Machine transformation:

[0054] First, a large gas mixing tank 2 is connected to the end of the gas path of the traditional machine. The tank body can be heated to 500-800℃. The outlet of the tank body is connected to the air inlet pipe 51 and the quartz liquid inlet pipe 52. The outer tube of the air inlet pipe 51 and the inner tube of the liquid inlet pipe 52 form a sleeve 5. The length of the air inlet pipe 51 extending into the furnace is about 15cm, and the length of the liquid inlet pipe 52 extending into the furnace is about 7cm, so as to realize the function of simultaneous air intake and liquid intake. Secondly, the thick tail gas pipe 31 is thinned, and the tail gas pipe 31 is changed from the original diameter of 50mm to 25-35mm, and the preferred diameter is 30mm. Its purpose is to increase the air pressure inside the furnace tube of the high-temperature furnace from 0.1mPa to 0.3-0.5mPa to form a pressure that promotes the deposition of single-walled carbon nanotubes on the top of the furnace tube of the high-temperature furnace. The improvement of the tube diameter increases the pressure inside the furnace body by slowing down the exhaust gas emission rate, thereby promoting the rapid deposition of single-walled carbon nanotubes.

[0055] (2) Experimental steps:

[0056] Liquid carbon source (including but not limited to toluene, benzyl alcohol, etc.), metal compound (including but not limited to cobaltocene, ferrocene, nickelocene, etc.), cocatalyst (including but not limited to thiophenol, selenophene, etc.) and modifier (including but not limited to ethanol, ethylene glycol, etc.) are made into dispersion according to a certain ratio. In addition, the dosage ratio of metal compound, liquid carbon source, cocatalyst and modifier is 2-6g: 60-180mL: 2-6mL: 20-25mL. Reducing gas methane and protective gas nitrogen need to enter the mixing tank together at a flow rate of 5000-7000sccm: 2500sccm for heating to ensure that the temperature and pressure rise to a certain level and can remain stable for a long time. Then open the outlet pipe valve in the mixing tank to allow the mixed gas to enter the furnace tube of the high-temperature furnace. The dispersion is introduced into a high-temperature furnace at 1150-1200°C at an injection speed of 180-210μL / min, and samples are collected every half hour to prevent excessive carbon tubes from being accumulated in the high-temperature zone for a long time and carbonized, which will lead to a decrease in the quality of single-walled carbon nanotubes. Since the generated single-walled carbon nanotube crude products are mainly deposited on the upper part of the furnace tube of the high-temperature furnace and inside the collection tank, the temperature is relatively low compared to the middle of the reactor. The generation temperature of single-walled carbon nanotubes is usually maintained at 1150-1200°C, but its deposition temperature needs to be lower, about 500-800°C. If the sample cannot be sampled in time, continuous deposition in the high-temperature zone will cause the product to become brittle, so samples need to be collected every half hour.

[0057] Next is the processing step of the crude product. The crude product is continuously calcined in air at 1000-1400°C for 1-2h to remove the amorphous carbon on the surface and increase the degree of graphitization of the product. Then, concentrated acid or concentrated hydrochloric acid is used to stir for a period of time at a certain temperature to remove metal impurities in the crude product. During the calcination process, the oxygen in the air provides sufficient supply to enable the amorphous carbon to be oxidized. Amorphous carbon is mainly composed of carbon elements, and when reacting with oxygen, carbon dioxide (CO2) or carbon monoxide (CO) is produced. These gases will be carried away, so that the amorphous carbon is removed. And during the calcination process, granular or flaky amorphous carbon is usually formed, so that the ratio of the peak area value of the G peak to the peak area value of the D peak in the Raman test index is low enough to reach a level of GD ratio (peak area ratio) greater than 90; and more surface area is exposed during the calcination process, which can increase the contact area between carbon and oxygen and improve the reaction efficiency. In order to completely remove the iron oxide impurities formed during the air calcination process, the crude product is continuously calcined at 1000-1400℃ with 200-400sccm of carbon monoxide (CO) for 1-2h. The iron oxide reacts with the carbon monoxide gas to generate metallic iron (Fe) and carbon dioxide (CO2). Carbon dioxide can be discharged along with the tail gas. In a 3-6M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution at a temperature of 30-40℃, stirring for 6-8h, iron (Fe) is more easily removed, while iron oxide (FeO2 or Fe2O3) is relatively difficult to be removed by hydrochloric acid. In contrast, iron oxide is not easily dissolved by hydrochloric acid due to its high stability. The reactivity of iron oxide is low. Although a certain degree of reaction may occur in a strong acid environment, the speed is slow, which will affect the speed and effect of removing metal impurities in single-walled carbon nanotubes to some extent. After carbon monoxide reacts chemically with iron oxide to generate elemental iron and carbon dioxide, the efficiency of metal removal during pickling is greatly improved.

[0058] Example

[0059] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0060] Example 1

[0061] First, the liquid carbon source (toluene), metal compound (ferrocene), co-catalyst (thiophenol) and modifier (ethanol) are made into a dispersion in a certain proportion. In addition, the dosage ratio of iron source, liquid carbon source, co-catalyst and modifier is 2g:30mL:2mL:25mL. The reducing gas methane and the protective gas nitrogen need to enter the mixing tank together at a flow rate of 5000sccm:2500sccm for heating to ensure that the temperature and pressure rise to a certain level and can remain stable for a long time. Then open the outlet pipe valve in the mixing tank to allow the mixed gas to enter the furnace tube of the high-temperature furnace. The dispersion is introduced into a high-temperature furnace of 1150-1200℃ at an injection speed of 200μL / min, and samples are collected every half an hour to prevent excessive carbon tubes from being accumulated in the high-temperature zone for a long time and carbonizing, resulting in a decrease in the quality of single-walled carbon nanotubes.

[0062] Next is the processing step of the crude product. First, the crude product is continuously calcined in air at 1400°C for 1 hour to remove amorphous carbon on the surface and increase the degree of graphitization of the product. In order to completely remove the iron oxide impurities formed during the air calcination process, the crude product is continuously calcined at 1400°C with 200sccm of carbon monoxide (CO) for 1 hour. The iron oxide reacts with carbon monoxide gas to generate metallic iron (Fe) and carbon dioxide (CO2). Carbon dioxide can be discharged along with the tail gas. Carbon monoxide reacts chemically with iron oxide to generate elemental iron and carbon dioxide. In a 3M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution at a temperature of 30°C, stir for 6 hours to remove metal impurities (iron impurities).

[0063] After weighing and Raman testing, it was found that 2.5068 g of single-walled net product could be produced in 6 h of Example 1, and the Raman G / D was as high as 234.5.

[0064] Embodiment 2:

[0065] First, the liquid carbon source (benzyl alcohol), metal compound (cobaltocene), cocatalyst (selenophene) and modifier (ethylene glycol) are made into a dispersion in a certain proportion. In addition, the ratio of the amount of metal compound, liquid carbon source, cocatalyst and modifier is 2g:40mL:2mL:25mL. The reducing gas methane and the protective gas nitrogen need to enter the mixing tank together at a flow rate of 5000sccm:2500sccm for heating to ensure that the temperature and pressure rise to a certain extent and can remain stable for a long time. Then open the outlet pipe valve in the mixing tank to allow the mixed gas to enter the furnace tube of the high-temperature furnace. The dispersion is introduced into a high-temperature furnace of 1150-1200℃ at an injection speed of 190μL / min, and samples are collected every half an hour to prevent excessive carbon tubes from being accumulated in the high-temperature zone for a long time and carbonizing, resulting in a decrease in the quality of single-walled carbon nanotubes.

[0066] Next is the processing step of the crude product. First, the crude product is continuously calcined in air at 1400°C for 1 hour to remove amorphous carbon on the surface and increase the degree of graphitization of the product. In order to completely remove the iron oxide impurities formed during the air calcination process, the crude product is continuously calcined at 1400°C with 200sccm of carbon monoxide (CO) for 1 hour. The iron oxide reacts with carbon monoxide gas to generate metal cobalt (Co) and carbon dioxide (CO2). Carbon dioxide can be discharged along with the tail gas. Carbon monoxide reacts chemically with iron oxide to generate elemental iron and carbon dioxide. In a 3M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution at a temperature of 30°C, stir for 6 hours to remove metal impurities (cobalt impurities).

[0067] After weighing and Raman testing, it was found that Example 2, Scheme 6h, could produce 2.1568g of single-walled net product, and the Raman G / D was as high as 201.5.

[0068] Embodiment 3:

[0069] First, the liquid carbon source (toluene), metal compound (nickelocene), co-catalyst (thiophenol) and modifier (ethylene glycol) are made into a dispersion in a certain proportion. In addition, the dosage ratio of metal compound, liquid carbon source, co-catalyst and modifier is 2g:50mL:2mL:25mL. The reducing gas methane and the protective gas nitrogen need to enter the mixing tank together at a flow rate of 5000sccm:2500sccm for heating to ensure that the temperature and pressure rise to a certain level and can remain stable for a long time. Then open the outlet pipe valve in the mixing tank to allow the mixed gas to enter the furnace tube of the high-temperature furnace. The dispersion is introduced into a high-temperature furnace of 1150-1200℃ at an injection speed of 180μL / min, and samples are collected every half an hour to prevent excessive carbon tubes from being accumulated in the high-temperature zone for a long time and carbonizing, resulting in a decrease in the quality of single-walled carbon nanotubes.

[0070] Next is the processing step of the crude product. First, the crude product is continuously calcined in air at 1400°C for 1 hour to remove amorphous carbon on the surface and increase the degree of graphitization of the product. In order to completely remove the iron oxide impurities formed during the air calcination process, the crude product is continuously calcined at 1400°C with 200sccm of carbon monoxide (CO) for 1 hour. The iron oxide reacts with carbon monoxide gas to generate metallic nickel (Ni) and carbon dioxide (CO2). Carbon dioxide can be discharged along with the tail gas. Carbon monoxide reacts chemically with iron oxide to generate elemental iron and carbon dioxide. In a 3M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution at a temperature of 30°C, stir for 6 hours to remove metal impurities (nickel impurities).

[0071] After weighing and Raman testing, it was found that the 6h of Example 3 could produce 1.9564g of single-walled net product, and the Raman G / D was as high as 161.5.

[0072] Comparative Example 1:

[0073] The scheme of comparative example 1 is the same as the method of embodiment 1, except that the reducing gas methane and the protective gas nitrogen do not need to enter the mixing tank together at a flow rate of 5000sccm:2500sccm for heating. In the scheme of comparative example 1, the experiment is directly carried out using a thick tail gas pipe.

[0074] After weighing and Raman testing, it was found that the comparative example 1 solution could produce 1.9026g of single-walled net product in 6 hours, and the Raman G / D was 103.2.

[0075] Comparative Example 2:

[0076] The scheme of comparative example 2 is the same as the method of example 1, except that the reducing gas methane and the protective gas nitrogen do not need to be introduced into the gas mixing tank at a flow rate of 5000 sccm:2500 sccm for heating. The difference is that the corresponding step of "calcining the crude product at 1400°C for 1 hour by introducing 200 sccm of carbon monoxide (CO)" is omitted.

[0077] After weighing and Raman testing, it was found that the Comparative Example 2 solution could produce 1.9008 g of single-walled carbon nanotubes in 6 hours, and the Raman G / D was 93.5. However, some residual metal impurities can be observed in the scanning electron microscope image of the single-walled carbon nanotubes.

[0078] Through the comparison between Example 1, Example 2 and Example 3, it can be observed that the production rate of single-walled carbon nanotubes in Example 1 is significantly greater than that in Example 2 and Example 3. The GD ratio between Example 1, Example 2 and Example 3 is basically maintained between 160-240, and there is not much difference. The growth condition of single-walled carbon nanotubes is based on the growth of tubular nanostructures of carbon sources on the surface of iron atoms or atomic groups. The higher the concentration of metallic iron-based compound materials in the solution, the more single-walled carbon nanotubes are grown. In Example 1, Example 2 and Example 3, the iron concentration in the dispersion of Example 1 is the highest. In addition, on the basis of maintaining the quality of single-walled carbon nanotubes, appropriately increasing the injection rate of the dispersion in the furnace body is more conducive to increasing the output of single-walled carbon nanotubes. (If the injection rate of the dispersion is too fast, the quality of the crude product will also be seriously reduced)

[0079] Comparative Example 1 is a single-walled carbon nanotube produced without heating the mixing tank. During the production process, the airflow is not stable and the pressure is insufficient. It can be found that its production rate is significantly lower than that of Example 1. The slight decrease in the GD ratio may be due to the unstable airflow in the device, which leads to a significant decrease in the deposition rate of the crude single-walled carbon nanotube. Comparative Example 2 reduces the relevant step of continuously calcining the crude product at 1400°C for 1h with 200sccm of carbon monoxide (CO) during the purification process. This method is not conducive to removing the excess iron oxide produced in the previous step of calcining in air at 1400°C for 1h to remove amorphous carbon. Therefore, more metal impurities can be found when taking a scanning electron microscope. The iron content contained in the single-walled carbon nanotube is too high, and the content of graphite carbon is relatively reduced, thereby significantly reducing the Raman value of the single-walled carbon nanotube.

[0080] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A method for preparing single-walled carbon nanotubes with high yield and purity, characterized in that: The following steps are involved: (1) preparing a dispersion liquid with a liquid carbon source, a metal compound, a co-catalyst and a modifier in a certain proportion; (2) The reducing gas methane and the protective gas enter the mixing tank together at a certain flow ratio for heating and mixing, and are introduced into the furnace tube of the high-temperature furnace after stabilization; (3) The dispersion is introduced into a high temperature furnace at a certain injection speed, and the crude product is collected every 20-40 minutes; (4) The crude product is calcined for a period of time to remove amorphous carbon on the surface; then, concentrated acid is used for stirring at a certain temperature for a period of time to remove metal impurities in the crude product.

2. The method for preparing single-walled carbon nanotubes with high yield and purity according to claim 1, characterized in that: The liquid carbon source is one or more of toluene and benzyl alcohol; the metal compound is one or more of cobaltocene, ferrocene and nickelocene; the co-catalyst is one or more of thiophenol and selenophene; the modifier is one or more of ethanol and ethylene glycol; the dosage ratio of the metal compound, liquid carbon source, co-catalyst and modifier is 2-6g:60-180mL:2-6mL:25mL.

3. The method for preparing single-walled carbon nanotubes with high yield and purity according to claim 1, characterized in that: The reducing gas is methane, the shielding gas is nitrogen, and the ratio of the reducing gas to the shielding gas is 5000-7000sccm:2500sccm.

4. The method for preparing single-walled carbon nanotubes with high yield and purity according to claim 1, characterized in that: The injection speed of the dispersion in step (3) is 180-210 μL / min; the furnace tube temperature of the high-temperature furnace is 1150-1200°C.

5. The method for preparing single-walled carbon nanotubes with high yield and purity according to claim 1, characterized in that: In the step (4), the crude product is calcined in air at 1000-1400° C.; the air oxidation time of the crude product is 1-2 hours.

6. The method for preparing single-walled carbon nanotubes with high yield and purity according to claim 5, characterized in that: After the amorphous carbon is removed in step (4), carbon monoxide is continued to be introduced for calcination.

7. The method for preparing single-walled carbon nanotubes with high yield and purity according to claim 6, characterized in that: The carbon monoxide is introduced at 200-400 sccm and calcined for 1-2 hours at a calcination temperature of 1000-1400°C.

8. The method for preparing single-walled carbon nanotubes with high yield and purity according to claim 1, characterized in that: The concentrated acid is concentrated hydrochloric acid or concentrated sulfuric acid; the stirring temperature is 30-40° C., and the stirring time is 6-8 hours.

9. A device for preparing single-walled carbon nanotubes with high yield and purity, comprising a gas cylinder, a gas mixing tank and a vertical tube furnace connected in sequence, and an injector connected to the vertical tube furnace, wherein the outlets of the gas mixing tank and the injector are both connected to the inlet of the vertical tube furnace, and the vertical tube furnace is provided with a tail gas pipe.

10. The device for preparing single-walled carbon nanotubes with high yield and purity according to claim 9, characterized in that: The heating temperature of the gas mixing tank is 500-800° C.; the diameter of the tail gas pipe is 25-35 mm.