Method for preparing modified carbon nanotubes and gel particles containing modified carbon nanotubes
By reinforcing gel particles with modified carbon nanotubes, the stability and hydrolysis resistance problems of the gel system in high-water-containing oil fields under high-temperature and high-salt conditions are solved, and better flooding effects and long-term plugging capabilities are achieved.
Patent Information
- Application Number
- CN202310479669.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-29
AI Technical Summary
In oil fields with high water content, the gel system is easily affected by temperature and salinity, resulting in degradation and viscosity reduction, making it difficult to achieve long-term sealing. In addition, acrylamide gel particles are easily hydrolyzed under high temperature and high salt conditions, affecting the flood control effect. .
Hydroxylated multi-walled carbon nanotubes are processed through multi-step modification to form modified carbon nanotubes, which are used to strengthen gel particles, form a spatial network structure, enhance mechanical strength and improve hydrolysis resistance.
The modified carbon nanotube-reinforced gel particles significantly improve the stability and hydrolysis resistance under high-temperature and high-salt conditions, extend the retention time of the expansion ratio, and enhance the flooding control effect.
Smart Images

Figure CN118851161A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of petroleum exploration, and in particular to gel particles for profile control or displacement control. Background Art
[0002] With the progress of oil exploration and development, most of my country's oil fields have entered a high water content period. How to make the water drive fluid flow efficiently circulate in high water content oil fields is the challenge facing the further exploitation of remaining oil. Gel system profile control / displacement control technology has become an important technical means to improve the recovery rate of major oil fields. However, during the development of oil fields, the gel system is easily affected by temperature, salinity, etc. and degrades, resulting in a decrease in viscosity, making it difficult to achieve long-term plugging of high permeability layers. Before being injected into the formation, the gel particles have formed a three-dimensional network structure, can absorb water and swell, and have a certain degree of deformability, which is conducive to entering the deep oil layer to expand the plugging range. Compared with the gel system, gel particles can effectively reduce the reservoir temperature, salinity, and the effects of shear and chromatographic separation during the injection process on its displacement effect, and can also avoid the damage of base fluid loss to the low permeability layer. However, the expansion of gel particles is greatly affected by temperature and salinity. Generally, the higher the temperature, the greater the expansion multiple of the gel particles, and the higher the salinity, the more its expansion is inhibited. In addition, acrylamide gel particles are easily hydrolyzed under high temperature and high salt conditions, and the particles become loose, resulting in poor flooding effect. Summary of the invention
[0003] One of the present inventions provides a method for preparing modified carbon nanotubes, which comprises the following steps:
[0004] 1) performing a first modification on the hydroxylated multi-walled carbon nanotubes using a silane coupling agent to obtain first modified carbon nanotubes;
[0005] 2) performing a second modification on the first modified carbon nanotubes using methyl acrylate to obtain second modified carbon nanotubes;
[0006] 3) performing a third modification on the second modified carbon nanotubes using ethylenediamine to obtain third modified carbon nanotubes;
[0007] 4) performing a fourth modification on the third modified carbon nanotubes using methyl acrylate to obtain fourth modified carbon nanotubes;
[0008] 5) subjecting the fourth modified carbon nanotube to a fifth modification using ethylenediamine to obtain a fifth modified carbon nanotube;
[0009] 6) The fifth modified carbon nanotube is subjected to a sixth modification using maleic acid to obtain a sixth modified carbon nanotube.
[0010] In a specific embodiment, in step 1), the hydroxylated multi-walled carbon nanotubes are dispersed in toluene and deoxygenated, and then the silane coupling agent is added dropwise, the temperature is raised to a first temperature, and the reaction is carried out at the first temperature for a first time to obtain a first reaction liquid, the first reaction liquid is vacuum filtered, and then washed with methanol, vacuum filtered again, and vacuum dried to obtain a first modified carbon nanotube.
[0011] In a specific embodiment, the mass ratio of the hydroxylated multi-walled carbon nanotubes to the silane coupling agent is 25:6.
[0012] In a specific embodiment, the silane coupling agent is γ-aminopropyltriethoxysilane.
[0013] In a specific embodiment, in step 2), the second modified carbon nanotubes are dispersed in methanol and deoxygenated, and then a methanol solution containing the methyl acrylate is added dropwise at a second temperature, the temperature is raised to a third temperature, and the reaction is carried out at the third temperature for a second period of time to obtain a second reaction liquid, the second reaction liquid is vacuum filtered, then washed with methanol, vacuum filtered again, and vacuum dried to obtain a second modified carbon nanotube.
[0014] In a specific embodiment, the mass ratio of the second modified carbon nanotubes to the methyl acrylate is 1:1.
[0015] In a specific embodiment, in step 3), the third modified carbon nanotubes are dispersed in methanol and deoxygenated, and then a methanol solution containing the ethylenediamine is added dropwise at a fourth temperature, the temperature is raised to a fifth temperature, and the reaction is carried out at the fifth temperature for a third time to obtain a third reaction liquid, the third reaction liquid is vacuum filtered, then washed with methanol, vacuum filtered again, and vacuum dried to obtain a third modified carbon nanotube.
[0016] In a specific embodiment, the mass ratio of the third modified carbon nanotube to the ethylenediamine is 1:1.
[0017] In a specific embodiment, in step 4), the first modified carbon nanotube is replaced with a third modified carbon nanotube, and step 2) is repeated.
[0018] In a specific embodiment, in step 5), the second modified carbon nanotube is replaced with a fourth modified carbon nanotube, and step 3) is repeated.
[0019] In a specific embodiment, in step 6), the fifth modified carbon nanotube is dispersed in dimethyl sulfoxide, deoxygenated, and then the dimethyl sulfoxide solution containing the maleic anhydride is added dropwise at a sixth temperature, the temperature is raised to a seventh temperature, and the reaction is carried out at the seventh temperature for a fourth time to obtain a sixth reaction liquid, the sixth reaction liquid is vacuum filtered, then washed with methanol, vacuum filtered again, and vacuum dried to obtain a sixth modified carbon nanotube.
[0020] In a specific embodiment, the mass ratio of the fifth modified carbon nanotube to the maleic anhydride is 5:4.
[0021] In a specific embodiment, the first temperature is 60 to 100°C, and the first time is 20 to 28 hours; the second temperature, the fourth temperature and the sixth temperature are independently 1 to 5°C; the third temperature and the fifth temperature are independently 20 to 30°C, and the second time and the third time are independently 18 to 30 hours; the seventh temperature is 20 to 60°C, and the fourth time is 12 to 30 hours; the vacuum drying conditions of step 1), step 2), step 3) and step 5) are independently 60 to 80°C for 24 to 36 hours.
[0022] The second aspect of the present invention provides a modified carbon nanotube-reinforced gel particle, the raw materials for preparing the modified carbon nanotube-reinforced gel particle include N,N-dimethylacrylamide, methacryloyloxyethyl dimethyl hexadecyl ammonium bromide, N,N-methylenebisacrylamide, azobisisobutylimidazoline hydrochloride and the sixth modified carbon nanotube prepared by the method described in any one of the embodiments of the present invention.
[0023] In a specific embodiment, the amount of N,N-dimethylacrylamide is 8 to 15 parts by mass; the amount of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide is 8 to 15 parts by mass; the amount of N,N-methylenebisacrylamide is 0.1 to 0.5 parts by mass; the amount of azobisisobutylimidazoline hydrochloride is 0.001 to 0.006 parts by mass; and the amount of the sixth modified carbon nanotube is 0.05 to 0.1 parts by mass.
[0024] In a specific embodiment, the modified carbon nanotube-reinforced gel particles are prepared by the following steps:
[0025] 1) mixing the sixth modified carbon nanotube, N,N-dimethylacrylamide, methacryloyloxyethyl dimethyl hexadecyl ammonium bromide and N,N-methylenebisacrylamide with water, and dispersing them uniformly to obtain a black solution;
[0026] 2) deoxygenating the black solution, adding the azobisisobutylimidazoline hydrochloride thereto, continuing to deoxygenate, and keeping the temperature at 40 to 60° C. for more than 4 hours to obtain a gel-like colloid;
[0027] 3) Cutting, granulating, drying and crushing the gel-like colloid to obtain the modified carbon nanotube-reinforced gel particles.
[0028] The third invention provides the use of the sixth modified carbon nanotube prepared by the method according to any one of the first invention or the modified carbon nanotube reinforced gel particles according to the second invention in profile control or flooding control.
[0029] Beneficial effects of the present invention:
[0030] 1) The modified carbon nanotube-reinforced gel particles of the present invention have a spatial network structure, and at the same time, the modified carbon nanotubes of the present invention are introduced into the spatial network structure, thereby enhancing the mechanical strength of the gel particles;
[0031] 2) The hydrolysis resistance of the modified carbon nanotube-enhanced gel particles of the present invention is significantly improved under high-temperature and high-salt oil reservoir conditions;
[0032] 3) The stability of the modified carbon nanotube-reinforced gel particles of the present invention under high temperature and high salt conditions is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Schematic diagram of the experimental setup for testing the steering pressure of gel particles is shown.
[0034] Figure 2 The steering pressure of the KYPAM solution is shown.
[0035] Figure 3 The turning pressure of the gel particle dispersion containing the modified carbon nanotube-reinforced gel particles prepared in Example 4 without aging is shown.
[0036] Figure 4 The turning pressure of the gel particle dispersion containing the modified carbon nanotube-reinforced gel particles prepared in Example 4 aged at 120° C. for 30 days is shown.
[0037] Figure 5 The turning pressure of the gel particle dispersion containing the modified carbon nanotube-reinforced gel particles prepared in Example 4 aged at 120° C. for 60 days is shown.
[0038] Figure 6 The expansion multiples of the modified carbon nanotube-reinforced gel particles prepared in Example 4 at different temperatures are shown.
[0039] Figure 7 The expansion multiples of the modified carbon nanotube-reinforced gel particles prepared in Example 4 at different mineralization degrees are shown. DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.
[0041] Unless otherwise specified, the raw materials used in the present invention can be purchased conventionally.
[0042] Hydroxylated multi-walled carbon nanotubes were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0043] Preparation of modified carbon nanotubes
[0044] Example 1
[0045] 1) Weigh 5.0 g of hydroxylated multi-walled carbon nanotubes and add them to 80 mL of toluene, and ultrasonically disperse the carbon nanotubes in the toluene to obtain a carbon nanotube dispersion; then transfer the mixture to a 250 mL three-necked flask, and introduce N2 to remove oxygen in the carbon nanotube dispersion; add 1.2 g of γ-aminopropyltriethoxysilane (KH-550) dropwise under magnetic stirring and N2 atmosphere; after the addition is completed, heat the mixture to 80° C. in a sealed container, and react at 80° C. for 24 h to obtain a first reaction solution; vacuum filter the first reaction solution, then wash it with methanol three times, vacuum filter it again, and vacuum dry it at 60° C. for 30 h to obtain a first modified carbon nanotube.
[0046] 2) Take 5.0g of the first modified carbon nanotubes and add them to 80mL of methanol, and use ultrasound to evenly disperse the first modified carbon nanotubes in the methanol to obtain a first modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the first modified carbon nanotube dispersion; control the temperature of the first modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and then add 40mL of a mixed solution of methyl acrylate (MA) and methanol (wherein the mass of MA is 5.0g) dropwise to the first modified carbon nanotube dispersion under stirring conditions; then heat the mixture to 25°C, and react at 25°C for 24h under stirring conditions to obtain a second reaction solution; vacuum filter the second reaction solution, then wash it with methanol repeatedly for 3 times, vacuum filter it again, and vacuum dry it at 60°C for 30h to obtain a second modified carbon nanotube.
[0047] 3) Take 5.0g of the second modified carbon nanotubes and add them to 80mL of methanol, and use ultrasound to evenly disperse the second modified carbon nanotubes in the methanol to obtain a second modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the second modified carbon nanotube dispersion; control the temperature of the second modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and add 40mL of a mixed solution of ethylenediamine (EDA) and methanol (wherein, the mass of EDA is 5.0g) dropwise to the second modified carbon nanotube dispersion under stirring conditions; then heat the mixture to 25°C, and react at 25°C for 24h under stirring conditions to obtain a third reaction liquid; vacuum filter the third reaction liquid, then wash it with methanol repeatedly for 3 times, vacuum filter it again, and vacuum dry it at 60°C for 30h to obtain a third modified carbon nanotube.
[0048] 4) replacing the first modified carbon nanotube with the third modified carbon nanotube, repeating step 2) to obtain a fourth modified carbon nanotube; replacing the second modified carbon nanotube with the fourth modified carbon nanotube, repeating step 3) to obtain a fifth modified carbon nanotube;
[0049] 5) Take 5.0g of the fifth modified carbon nanotube and add it to 80mL dimethyl sulfoxide (DMSO), and use ultrasound to make the fifth modified carbon nanotube evenly dispersed in the DMSO to obtain a fifth modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the fifth modified carbon nanotube dispersion; control the temperature of the fifth modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and then add 40mL of a mixed solution of maleic anhydride (MAH) and DMSO (wherein, the mass of MAH is 4.0g) to the fifth modified carbon nanotube dispersion under stirring; then heat it to 60°C, and react at 60°C for 12h under stirring to obtain a sixth reaction liquid; after cooling the sixth reaction liquid to room temperature, vacuum filtration is performed to remove unreacted monomers, and then washed with methanol 3 times, vacuum filtered again, and vacuum dried at 60°C for 30h to obtain a sixth modified carbon nanotube.
[0050] Example 2
[0051] 1) Weigh 5.0 g of hydroxylated multi-walled carbon nanotubes and add them to 80 mL of toluene, and ultrasonically disperse the carbon nanotubes in the toluene to obtain a carbon nanotube dispersion; then transfer the mixture to a 250 mL three-necked flask, and introduce N2 to remove oxygen in the carbon nanotube dispersion; add 1.2 g of γ-aminopropyltriethoxysilane (KH-550) dropwise under magnetic stirring and N2 atmosphere; after the addition is completed, heat the mixture to 100° C. in a sealed manner, and react at 100° C. for 20 h to obtain a first reaction liquid; vacuum filter the first reaction liquid, then wash it repeatedly with methanol for 3 times, vacuum filter it again, and vacuum dry it at 80° C. for 24 h to obtain a first modified carbon nanotube.
[0052] 2) Take 5.0g of the first modified carbon nanotubes and add them to 80mL of methanol, and use ultrasound to evenly disperse the first modified carbon nanotubes in the methanol to obtain a first modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the first modified carbon nanotube dispersion; control the temperature of the first modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and then add 40mL of a mixed solution of methyl acrylate (MA) and methanol (wherein the mass of MA is 5.0g) dropwise to the first modified carbon nanotube dispersion under stirring; then heat it to 30°C, and react at 30°C for 18h under stirring to obtain a second reaction solution; vacuum filter the second reaction solution, then wash it with methanol repeatedly for 3 times, vacuum filter it again, and vacuum dry it at 65°C for 24h to obtain a second modified carbon nanotube.
[0053] 3) Take 5.0g of the second modified carbon nanotubes and add them to 80mL of methanol, and use ultrasound to evenly disperse the second modified carbon nanotubes in the methanol to obtain a second modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the second modified carbon nanotube dispersion; control the temperature of the second modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and add 40mL of a mixed solution of ethylenediamine (EDA) and methanol (wherein, the mass of EDA is 5.0g) dropwise to the second modified carbon nanotube dispersion under stirring conditions; then heat the mixture to 30°C, and react at 30°C for 18h under stirring conditions to obtain a third reaction liquid; vacuum filter the third reaction liquid, then wash it with methanol repeatedly for 3 times, vacuum filter it again, and vacuum dry it at 65°C for 24h to obtain a third modified carbon nanotube.
[0054] 4) replacing the first modified carbon nanotube with the third modified carbon nanotube, repeating step 2) to obtain a fourth modified carbon nanotube; replacing the second modified carbon nanotube with the fourth modified carbon nanotube, repeating step 3) to obtain a fifth modified carbon nanotube;
[0055] 5) Take 5.0g of the fifth modified carbon nanotube and add it to 80mL dimethyl sulfoxide (DMSO), and use ultrasound to make the fifth modified carbon nanotube evenly dispersed in the DMSO to obtain a fifth modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the fifth modified carbon nanotube dispersion; control the temperature of the fifth modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and then add 40mL of a mixed solution of maleic anhydride (MAH) and DMSO (wherein, the mass of MAH is 4.0g) to the fifth modified carbon nanotube dispersion under stirring; then heat it to 30°C, and react at 30°C for 18h under stirring to obtain a sixth reaction liquid; after cooling the sixth reaction liquid to room temperature, vacuum filter it to remove unreacted monomers, then wash it with methanol 3 times, vacuum filter it again, and vacuum dry it at 65°C for 24h to obtain a sixth modified carbon nanotube.
[0056] Example 3
[0057] 1) Weigh 5.0 g of hydroxylated multi-walled carbon nanotubes and add them to 80 mL of toluene, and ultrasonically disperse the carbon nanotubes in the toluene to obtain a carbon nanotube dispersion; then transfer the mixture to a 250 mL three-necked flask, and introduce N2 to remove oxygen in the carbon nanotube dispersion; add 1.2 g of γ-aminopropyltriethoxysilane (KH-550) dropwise under magnetic stirring and N2 atmosphere; after the addition is completed, heat the mixture to 60°C in a sealed manner, and react at 60°C for 28 hours to obtain a first reaction liquid; vacuum filter the first reaction liquid, then wash it with methanol repeatedly for 3 times, vacuum filter it again, and vacuum dry it at 60°C for 36 hours to obtain a first modified carbon nanotube.
[0058] 2) Take 5.0g of the first modified carbon nanotubes and add them to 80mL of methanol, and use ultrasound to evenly disperse the first modified carbon nanotubes in the methanol to obtain a first modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the first modified carbon nanotube dispersion; control the temperature of the first modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and then add 40mL of a mixed solution of methyl acrylate (MA) and methanol (wherein the mass of MA is 5.0g) dropwise to the first modified carbon nanotube dispersion under stirring; then heat it to 20°C, and react at 20°C for 30h under stirring to obtain a second reaction solution; vacuum filter the second reaction solution, then wash it with methanol repeatedly for 3 times, vacuum filter it again, and vacuum dry it at 60°C for 36h to obtain a second modified carbon nanotube.
[0059] 3) Take 5.0g of the second modified carbon nanotubes and add them to 80mL of methanol, and use ultrasound to evenly disperse the second modified carbon nanotubes in the methanol to obtain a second modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the second modified carbon nanotube dispersion; control the temperature of the second modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and add 40mL of a mixed solution of ethylenediamine (EDA) and methanol (wherein, the mass of EDA is 5.0g) dropwise to the second modified carbon nanotube dispersion under stirring conditions; then heat the mixture to 20°C, and react at 20°C for 30h under stirring conditions to obtain a third reaction liquid; vacuum filter the third reaction liquid, then wash it with methanol repeatedly for 3 times, vacuum filter it again, and vacuum dry it at 60°C for 36h to obtain a third modified carbon nanotube.
[0060] 4) replacing the first modified carbon nanotube with the third modified carbon nanotube, repeating step 2) to obtain a fourth modified carbon nanotube; replacing the second modified carbon nanotube with the fourth modified carbon nanotube, repeating step 3) to obtain a fifth modified carbon nanotube;
[0061] 5) Take 5.0g of the fifth modified carbon nanotube and add it to 80mL dimethyl sulfoxide (DMSO), and use ultrasound to make the fifth modified carbon nanotube evenly dispersed in the DMSO to obtain a fifth modified carbon nanotube dispersion; then transfer it to a 250mL three-necked flask, and introduce N2 to remove oxygen in the fifth modified carbon nanotube dispersion; control the temperature of the fifth modified carbon nanotube dispersion at 1 to 5°C with an ice bath, and then add 40mL of a mixed solution of maleic anhydride (MAH) and DMSO (wherein, the mass of MAH is 4.0g) to the fifth modified carbon nanotube dispersion under stirring; then heat it to 20°C, and react at 20°C for 30h under stirring to obtain a sixth reaction liquid; after cooling the sixth reaction liquid to room temperature, vacuum filter it to remove unreacted monomers, then wash it with methanol 3 times, vacuum filter it again, and vacuum dry it at 60°C for 36h to obtain a sixth modified carbon nanotube.
[0062] Preparation of modified carbon nanotube-reinforced gel particles
[0063] Example 4
[0064] A modified carbon nanotube reinforced gel particle is prepared from the following raw material components: 0.05 g of the sixth modified carbon nanotube prepared in Example 1; 10 g of N,N-dimethylacrylamide; 15 g of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide; 0.1 g of N,N-methylenebisacrylamide; 0.001 g of azobisisobutylimidazoline hydrochloride; and 75 g of pure water.
[0065] 1) adding 0.05 g of the sixth modified carbon nanotube, 10 g of N,N-dimethylacrylamide, 15 g of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide and 0.1 g of N,N-methylenebisacrylamide to pure water, and performing ultrasonication to obtain a black solution;
[0066] 2) N2 was passed through the black solution to deoxygenate for 30 minutes, and then 0.001 g of azobisisobutylimidazoline hydrochloride was added, and N2 was continued to be passed through for 30 minutes, and then the temperature was raised to 50°C and kept warm for 4 hours to obtain a uniform black gel-like colloid;
[0067] 3) The black gel-like colloid is cut, granulated, dried at 80° C. for 10 h, crushed and sieved according to needs to obtain modified carbon nanotube-reinforced gel particles.
[0068] Example 5
[0069] A modified carbon nanotube reinforced gel particle is prepared from the following raw material components: 0.1 g of the sixth modified carbon nanotube prepared in Example 1; 15 g of N,N-dimethylacrylamide; 8 g of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide; 0.5 g of N,N-methylenebisacrylamide; 0.003 g of azobisisobutylimidazoline hydrochloride; and 74 g of pure water.
[0070] 1) adding 0.1 g of the sixth modified carbon nanotube, 15 g of N,N-dimethylacrylamide, 8 g of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide and 0.5 g of N,N-methylenebisacrylamide to pure water, and performing ultrasonication to obtain a black solution;
[0071] 2) N2 was passed through the black solution to deoxygenate for 30 minutes, and then 0.003 g of azobisisobutylimidazoline hydrochloride was added, and N2 was continued to be passed through for 30 minutes, and then the temperature was raised to 40°C and kept warm for 4 hours to obtain a black gel-like colloid;
[0072] 3) The black gel-like colloid is cut, granulated, dried at 80° C. for 10 h, crushed and sieved according to needs to obtain modified carbon nanotube-reinforced gel particles.
[0073] Example 6
[0074] A modified carbon nanotube reinforced gel particle is prepared from the following raw material components: 0.05 g of the sixth modified carbon nanotube prepared in Example 1; 8 g of N,N-dimethylacrylamide; 8 g of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide; 0.1 g of N,N-methylenebisacrylamide; 0.006 g of azobisisobutylimidazoline hydrochloride; and 84 g of pure water.
[0075] 1) adding 0.05 g of the sixth modified carbon nanotube, 8 g of N,N-dimethylacrylamide, 8 g of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide and 0.1 g of N,N-methylenebisacrylamide to pure water, and performing ultrasonication to obtain a black solution;
[0076] 2) N2 was passed through the black solution to deoxygenate for 30 minutes, and then 0.006 g of azobisisobutylimidazoline hydrochloride was added, and N2 was continued to be passed through for 30 minutes, and then the temperature was raised to 60°C and kept warm for 4 hours to obtain a uniform black gel-like colloid;
[0077] 3) The black gel-like colloid is cut, granulated, dried at 80° C. for 10 h, crushed and sieved according to needs to obtain modified carbon nanotube-reinforced gel particles.
[0078] Example 7
[0079] A modified carbon nanotube reinforced gel particle is prepared from the following raw material components: 0.1 g of the sixth modified carbon nanotube prepared in Example 1; 15 g of N,N-dimethylacrylamide; 15 g of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide; 0.2 g of N,N-methylenebisacrylamide; 0.001 g of azobisisobutylimidazoline hydrochloride; and 70 g of pure water.
[0080] 1) adding 0.1 g of the sixth modified carbon nanotube, 15 g of N,N-dimethylacrylamide, 15 g of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide and 0.2 g of N,N-methylenebisacrylamide to pure water, and performing ultrasonication to obtain a black solution;
[0081] 2) N2 was passed through the black solution to deoxygenate for 30 minutes, and then 0.001 g of azobisisobutylimidazoline hydrochloride was added, and N2 was continued to be passed through for 30 minutes, and then the temperature was raised to 40°C and kept warm for 4 hours to obtain a uniform black gel-like colloid;
[0082] 3) The black gel-like colloid is cut, granulated, dried at 80° C. for 10 h, crushed and sieved according to needs to obtain modified carbon nanotube-reinforced gel particles.
[0083] Example 8
[0084] The sixth modified carbon nanotube prepared in Example 1 is replaced by the sixth modified carbon nanotube prepared in Example 2, and the rest is the same as in Example 4.
[0085] Example 9
[0086] The sixth modified carbon nanotube prepared in Example 1 was replaced by the sixth modified carbon nanotube prepared in Example 3, and the rest was the same as in Example 4.
[0087] Comparative Example 1
[0088] The sixth modified carbon nanotube prepared in Example 1 was replaced with hydroxylated multi-walled carbon nanotubes, and the rest was the same as in Example 4.
[0089] In particular, after the ultrasonic treatment in step 1), the hydroxylated multi-walled carbon nanotubes in the black liquid are separated due to the sedimentation of the black hydroxylated multi-walled carbon nanotubes; after the gel-like colloid is obtained in step 2), the black hydroxylated multi-walled carbon nanotubes are obviously gathered at the bottom of the colloid, while there are almost no black hydroxylated multi-walled carbon nanotubes at the top. This indicates that the hydroxylated multi-walled carbon nanotubes cannot be uniformly chemically grafted into the colloid, nor can they be uniformly incorporated into the colloid.
[0090] Comparative Example 2
[0091] The sixth modified carbon nanotube prepared in Example 1 is replaced by the first modified carbon nanotube prepared in Example 1, and the other steps are the same as those in Example 4.
[0092] Among them, after the ultrasonic treatment in step 1), the first modified carbon nanotubes in the black liquid were stratified due to the sedimentation of the black first modified carbon nanotubes; after the gel-like colloid was obtained in step 2), the black first modified carbon nanotubes were obviously gathered at the bottom of the colloid, and there were almost no black first modified carbon nanotubes at the top. This shows that the first modified carbon nanotubes cannot be uniformly chemically grafted into the colloid, nor can they be uniformly incorporated into the colloid, but the uniformity is improved compared with before the modification.
[0093] Comparative Example 3
[0094] The sixth modified carbon nanotube prepared in Example 1 was replaced by the second modified carbon nanotube prepared in Example 1, and the rest was the same as in Example 4.
[0095] Among them, after the ultrasonic treatment in step 1), the second modified carbon nanotubes in the black liquid were stratified due to the sedimentation of the black second modified carbon nanotubes; after the gel-like colloid was obtained in step 2), the black second modified carbon nanotubes were obviously gathered at the bottom of the colloid, and there were almost no black second modified carbon nanotubes at the top. This shows that the second modified carbon nanotubes cannot be uniformly chemically grafted into the colloid, and are also uniformly incorporated into the colloid, but the uniformity is improved compared with the first modified carbon nanotubes.
[0096] Comparative Example 4
[0097] The sixth modified carbon nanotube prepared in Example 1 is replaced by the third modified carbon nanotube prepared in Example 1, and the rest is the same as in Example 4.
[0098] Among them, after the end of the ultrasound, the third modified carbon nanotubes in the black liquid in step 1) are stratified due to the sedimentation of the black third modified carbon nanotubes; after the gel-like colloid is obtained in step 2), the black third modified carbon nanotubes are obviously gathered at the bottom of the colloid, and there are almost no black third modified carbon nanotubes in the upper part. This shows that the third modified carbon nanotubes cannot be uniformly chemically grafted into the colloid, and are also uniformly incorporated into the colloid, but the uniformity is improved compared with the second modified carbon nanotubes.
[0099] Comparative Example 5
[0100] The sixth modified carbon nanotube prepared in Example 1 is replaced by the fourth modified carbon nanotube prepared in Example 1, and the rest is the same as in Example 4.
[0101] Among them, after the ultrasound treatment in step 1), the fourth modified carbon nanotubes in the black liquid were separated due to the sedimentation of the black fourth modified carbon nanotubes; after the gel-like colloid was obtained in step 2), the black fourth modified carbon nanotubes were obviously gathered at the bottom of the colloid, and there were almost no black fourth modified carbon nanotubes at the top. This shows that the fourth modified carbon nanotubes cannot be uniformly chemically grafted into the colloid, and are also uniformly incorporated into the colloid, but the uniformity is improved compared with the third modified carbon nanotubes.
[0102] Comparative Example 6
[0103] The sixth modified carbon nanotube prepared in Example 1 is replaced by the fifth modified carbon nanotube prepared in Example 1, and the rest is the same as Example 4.
[0104] Among them, after the ultrasonic treatment in step 1), the fifth modified carbon nanotubes in the black liquid slightly precipitate and gradually gather to the bottom; after the gel-like colloid is obtained in step 2), the fifth modified carbon nanotubes are gradually distributed in the colloid from top to bottom from small to large. This indicates that the fifth modified carbon nanotubes cannot be uniformly chemically grafted into the colloid, and are also uniformly incorporated into the colloid, but the uniformity is improved compared with the fourth modified carbon nanotubes.
[0105] Performance Evaluation
[0106] (1) Strength of gel particles
[0107] The principle of testing the strength of gel particles is: when the pre-crosslinked gel particles pass through the screen, they will block the screen, resulting in a decrease in flow and an increase in injection pressure; when the pressure increases to the turning pressure of the pre-crosslinked gel particles, the gel particles blocking the screen will deform and break through the screen, and the flow will return to normal. The greater the strength of the gel particles, the greater the turning pressure.
[0108] Using mineralization degree 1×10 4 5000 mg / L KYPAM solution (molecular weight: 10 million) was prepared with 1000 mg / L NaCl aqueous solution.
[0109] The modified carbon nanotube-enhanced gel particles prepared in Examples 4 to 9 were dispersed in a 1×10 4 A gel particle dispersion was prepared in a sodium chloride aqueous solution with a concentration of 5000 mg / L, and KYPAM with a molecular weight of 10 million was added thereto.
[0110] The KYPAM solution was directly subjected to pressure steering without aging; three portions of the gel particle dispersion of each embodiment were prepared, one portion was directly subjected to pressure steering without aging, one portion was subjected to pressure steering after aging at 120°C for 30 days, and one portion was subjected to pressure steering after aging at 120°C for 60 days.
[0111] The steering pressure of gel particles was tested using an improved TGU experimental device. The schematic diagram of the experimental device is shown in Figure 1 As shown. The TGU value represents the relative resistance of the KYPAM solution or gel particle dispersion to pass through the screen. A certain pressure is applied to the intermediate container through a nitrogen bottle, and the flow rate of the KYPAM solution or gel particle dispersion under different pressures is tested, and the TGU value is calculated according to formula 1). The specific steps are as follows:
[0112] I) Install the steering pressure test equipment, in which adjacent screens are staggered 45° from each other;
[0113] II) adding the prepared KYPAM solution into the intermediate container and adjusting the pressure to 20 kPa through a pressure reducing valve;
[0114] III) Open the outlet, start counting when liquid starts to flow out of the outlet, and record the liquid volume after 5 minutes;
[0115] IV) adjusting the pressure reducing valve to increase the pressure to 60 kPa, 100 kPa, 150 kPa and 200 kPa respectively, and testing the liquid output volume in 5 min under different pressures;
[0116] V) taking out the sieve, washing it and putting it back in, then adding the KYPAM-gel particle composite system into the intermediate container, and repeating the experimental steps II) to V);
[0117] VI) Based on the relationship between the TGU value and flow rate of the system under different pressures, the turning pressure of the gel particles is obtained.
[0118]
[0119] Where: Q p ——KYPAM solution flow rate, mL / min;
[0120] Q g ——Flow rate of KYPAM-gel particle composite system, mL / min;
[0121] △P p ——KYPAM solution displacement pressure difference, kPa;
[0122] △P g ——Displacement pressure difference of KYPAM-gel particle composite system, kPa.
[0123] in, Figure 2 The steering pressure of the KYPAM solution is shown to be 121.7 kPa; Figure 3 The turning pressure of the gel particle dispersion containing the modified carbon nanotube-reinforced gel particles prepared in Example 4 without aging is shown to be 123.1 kPa; Figure 4 shows the turning pressure of a gel particle dispersion containing modified carbon nanotube-reinforced gel particles prepared in Example 4 aged at 120° C. for 30 days; Figure 5 The turning pressure of the gel particle dispersion containing the modified carbon nanotube-reinforced gel particles prepared in Example 4 aged at 120°C for 60 days is 127.6 kPa. It can be seen that after aging for 60 days, the strength is still higher than the initial strength, so the modified carbon nanotube-reinforced gel particles show higher strength and stability.
[0124] (2) Heat and salt resistance
[0125] The modified carbon nanotube-enhanced gel particles prepared in Examples 4 to 9 were dispersed in a 1×10 4 mg / L sodium chloride aqueous solution to prepare a gel particle dispersion. Four portions of the gel particle dispersion of each example were prepared and placed at 30°C, 90°C, 120°C and 150°C, respectively, and the expansion multiples (i.e., water absorption multiples) were measured at 0h, 5h, 10h, 24h, 10d, 30d, 60d, 90d and 90d, where: Figure 6 The expansion multiples of the modified carbon nanotube-enhanced gel particles at different temperatures prepared in Example 4. The calculation formula of the water absorption of the gel particles per unit mass is shown in Formula 2).
[0126]
[0127] Where: m L ——The mass of gel particles after absorbing water and swelling, g;
[0128] m s ——The mass of gel particles before swelling due to water absorption, g;
[0129] A——Expansion multiple of gel particles per unit mass, g / g.
[0130] from Figure 6 It can be seen that with the increase of temperature, the expansion multiple of gel particles increases. With the extension of aging experiment, the expansion multiple of gel particles increases first and then tends to be stable. When the time reaches 120d, the mass of gel particles remains unchanged.
[0131] The modified carbon nanotube-enhanced gel particles prepared in Examples 4 to 9 were dispersed in a 1×10 4mg / L sodium chloride aqueous solution, mineralization degree 5×10 4 mg / L sodium chloride aqueous solution, mineralization degree 10×10 4 mg / L sodium chloride aqueous solution, mineralization degree 20×10 4 The obtained gel particle dispersion was placed at 150°C and the expansion multiples were measured at 0h, 5h, 10h, 24h, 10d, 30d, 60d and 90d, where: Figure 7 The expansion multiples of the modified carbon nanotube-enhanced gel particles at different mineralization degrees prepared in Example 4. The calculation formula of the water absorption of the unit mass of the gel particles is shown in Formula 2).
[0132] from Figure 7 It can be seen that at a high temperature of 150°C, the expansion multiple of the gel particles decreases with the increase of mineralization, but at a mineralization of 20×10 4 It can still expand 28 times at 100 mg / L, thus showing good temperature and salt resistance.
[0133] (3) Oil displacement experiment
[0134] Using mineralization degree 20×10 4 mg / L NaCl aqueous solution was used to prepare a gel particle dispersion with a concentration of 5000 mg / L.
[0135] According to the reservoir data provided by an oil field, a parallel core flooding experiment was conducted to simulate reservoir conditions (temperature 120℃, salinity 200000mg / LNaCl). First, the basic parameters of the core were measured, then saturated with crude oil, and the oil saturation was recorded; then water flooding was performed at a rate of 0.5mL / min until the water content reached 98%; after the water flooding was completed, 0.3PV gel particle dispersion was injected at a rate of 0.5mL / min; then water flooding was performed at a rate of 0.5mL / min, and finally the recovery rate of high and low permeability cores was recorded.
[0136] Among them, Table 1 shows the displacement results of the gel particle dispersion prepared using the modified carbon nanotube enhanced gel particles prepared in Example 4. According to Table 1, when the permeability difference is between 6.5-27.2, the low permeability layer is not activated during the water flooding process; after the gel particle dispersion is injected, the low permeability layer is activated. When the difference is 27.2, the low permeability core recovery rate can still reach 7.5%, indicating that the gel particles can well expand the swept volume of the injected water in the oil layer, so that the injected water can reach the deep part of the oil layer zone and better activate the function of the low permeability layer.
[0137] Table 1. Core parameters and recovery rate
[0138]
[0139] In summary, the modified carbon nanotube-reinforced gel particles of the present invention significantly improve the stability of the gel particles under high temperature and high salt conditions due to the addition of the sixth modified carbon nanotubes.
[0140] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, the subject matter, spirit and scope of the present invention may be varied to accommodate specific situations, materials, material combinations and methods. All of these changes are included within the scope of the claims of the present invention.
Claims
1. A method for preparing modified carbon nanotubes, comprising the following steps: 1) performing a first modification on the hydroxylated multi-walled carbon nanotubes using a silane coupling agent to obtain first modified carbon nanotubes; 2) performing a second modification on the first modified carbon nanotubes using methyl acrylate to obtain second modified carbon nanotubes; 3) performing a third modification on the second modified carbon nanotubes using ethylenediamine to obtain third modified carbon nanotubes; 4) performing a fourth modification on the third modified carbon nanotubes using methyl acrylate to obtain fourth modified carbon nanotubes; 5) subjecting the fourth modified carbon nanotube to a fifth modification using ethylenediamine to obtain a fifth modified carbon nanotube; 6) The fifth modified carbon nanotube is subjected to a sixth modification using maleic acid to obtain a sixth modified carbon nanotube.
2. The method according to claim 1, characterized in that: In step 1), the hydroxylated multi-walled carbon nanotubes are dispersed in toluene, deoxygenated, and then the silane coupling agent is added dropwise, the temperature is raised to a first temperature, and the reaction is carried out at the first temperature for a first time to obtain a first reaction liquid, the first reaction liquid is vacuum filtered, and then washed with methanol, vacuum filtered again, and vacuum dried to obtain a first modified carbon nanotube; Preferably, the mass ratio of the hydroxylated multi-walled carbon nanotubes to the silane coupling agent is 25:
6.
3. The method according to claim 1, characterized in that In step 2), the second modified carbon nanotubes are dispersed in methanol, deoxygenated, and then the methanol solution containing the methyl acrylate is added dropwise at a second temperature, the temperature is raised to a third temperature, and the reaction is carried out at the third temperature for a second time to obtain a second reaction liquid, the second reaction liquid is vacuum filtered, and then washed with methanol, vacuum filtered again, and vacuum dried to obtain second modified carbon nanotubes; Preferably, the mass ratio of the second modified carbon nanotubes to the methyl acrylate is 1:
1.
4. The method according to claim 1, characterized in that: In step 3), the third modified carbon nanotubes are dispersed in methanol, deoxygenated, and then the methanol solution containing ethylenediamine is added dropwise at a fourth temperature, the temperature is raised to a fifth temperature, and the reaction is carried out at the fifth temperature for a third time to obtain a third reaction liquid, the third reaction liquid is vacuum filtered, and then washed with methanol, vacuum filtered again, and vacuum dried to obtain a third modified carbon nanotube; Preferably, the mass ratio of the third modified carbon nanotube to the ethylenediamine is 1:
1.
5. The method according to claim 3, characterized in that: In step 4), the first modified carbon nanotube is replaced with the third modified carbon nanotube, and step 2) is repeated.
6. The method according to claim 4, characterized in that In step 5), the second modified carbon nanotube is replaced with the fourth modified carbon nanotube, and step 3) is repeated.
7. The method according to claim 1, characterized in that In step 6), the fifth modified carbon nanotubes are dispersed in dimethyl sulfoxide, deoxygenated, and then the dimethyl sulfoxide solution containing maleic anhydride is added dropwise at a sixth temperature, the temperature is raised to a seventh temperature, and the reaction is carried out at the seventh temperature for a fourth time to obtain a sixth reaction liquid, the sixth reaction liquid is vacuum filtered, and then washed with methanol, vacuum filtered again, and vacuum dried to obtain a sixth modified carbon nanotube; Preferably, the mass ratio of the fifth modified carbon nanotube to the maleic anhydride is 5:
4.
8. The method according to claim 1, characterized in that The first temperature is 60 to 100° C., and the first time period is 20 to 28 hours; The second temperature, the fourth temperature and the sixth temperature are independently 1 to 5°C; The third temperature and the fifth temperature are independently 20 to 30° C., and the second time period and the third time period are independently 18 to 30 h; The seventh temperature is 20 to 60° C., and the fourth duration is 12 to 30 hours; The vacuum drying conditions of step 1), step 2), step 3) and step 5) are independently 60 to 80° C. for 24 to 36 hours.
9. A modified carbon nanotube reinforced gel particle, wherein the raw materials for preparing the modified carbon nanotube include N,N-dimethylacrylamide, methacryloyloxyethyl dimethyl hexadecyl ammonium bromide, N,N-methylenebisacrylamide, azobisisobutylimidazoline hydrochloride and the sixth modified carbon nanotube prepared by the method according to any one of claims 1 to 8; Preferably, the amount of N,N-dimethylacrylamide is 8 to 15 parts by mass; the amount of methacryloyloxyethyl dimethyl hexadecyl ammonium bromide is 8 to 15 parts by mass; the amount of N,N-methylenebisacrylamide is 0.1 to 0.5 parts by mass; the amount of azobisisobutylimidazoline hydrochloride is 0.001 to 0.006 parts by mass; the amount of the sixth modified carbon nanotube is 0.05 to 0.1 parts by mass; Preferably, the modified carbon nanotube-reinforced gel particles are prepared by the following steps: 1) mixing the sixth modified carbon nanotube, N,N-dimethylacrylamide, methacryloyloxyethyl dimethyl hexadecyl ammonium bromide and N,N-methylenebisacrylamide with water, and dispersing them uniformly to obtain a black solution; 2) deoxygenating the black solution, adding the azobisisobutylimidazoline hydrochloride thereto, continuing to deoxygenate, and keeping the temperature at 40 to 60° C. for more than 4 hours to obtain a gel-like colloid; 3) Cutting, granulating, drying and crushing the gel-like colloid to obtain the modified carbon nanotube-reinforced gel particles.
10. Use of the sixth modified carbon nanotube prepared by the method according to any one of claims 1 to 8 or the modified carbon nanotube-reinforced gel particles according to claim 9 in profile control or flooding control.
Citation Information
Patent Citations
Method for preparing carbon nanotube composite conductive hydrogel coating modified electrode
CN103196965A
Modified carbon nanotube cross-linking agent, hydrogel plugging agent and preparation method
CN111434713A
Carbon nanotube hybrid pre-crosslinked gel particles for deep profile control and flooding of oil reservoir and preparation method thereof
CN111533863A
Hyperbranched polymer based on carbon nanotube and preparation method thereof
CN113024747A
Preparation method of modified carbon nanotube and application of modified carbon nanotube in tire tread rubber
CN115594887A