Method for purifying graphite in lithium extraction slag of waste lithium iron phosphate battery positive and negative electrode mixture

The graphite in the positive and negative electrode mixture of used lithium iron phosphate batteries is purified through steps such as drying, crushing, water washing and acid washing, which solves the problem of immature recycling of negative electrode materials for lithium ion batteries and realizes the purification of high-purity graphite and the utilization of resources. Maximizing utilization promotes closed-circuit circulation and environmental protection of lithium-ion batteries.

CN118851168AInactive Publication Date: 2024-10-29GANNAN NORMAL UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410855246.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing technology is immature in recycling waste lithium-ion battery anode materials, resulting in resource waste and environmental pollution, and there is a lack of effective purification methods to achieve closed-circuit recycling of lithium-ion batteries.

Method used

A process including drying, crushing, water washing, acid leaching, mixed acid washing and high temperature calcination is used to purify the graphite in the positive and negative electrode mixture of used lithium iron phosphate batteries, and is treated with a mixed acid of hydrochloric acid, hydrogen peroxide and hydrofluoric acid. , to achieve high-temperature roasting and purification of graphite.

Benefits of technology

It achieves the high-purity purification of graphite (up to 99.8%), maximizes the utilization of resources and protects the environment, and provides graphite regeneration and recycling and multiple application paths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851168A_ABST
    Figure CN118851168A_ABST
Patent Text Reader

Abstract

The invention discloses a method for purifying graphite in waste lithium iron phosphate battery positive and negative electrode mixture lithium extraction slag. The method comprises the following steps: step 1, drying and crushing the waste lithium iron phosphate battery positive and negative electrode mixture lithium extraction slag; step 2, washing the lithium extraction slag obtained in the step 1 with water and filtering; 3, placing the filter residues obtained in the step 2 in a hydrochloric acid solution for leaching and filtering; step 4, leaching the filter residue obtained in the step 3 in a mixed acid composed of hydrochloric acid, hydrogen peroxide and hydrofluoric acid, filtering, washing and drying; and fifthly, the leaching product obtained in the fourth step is placed in a muffle furnace to be calcined, and an obtained high-temperature roasting product is the graphite obtained after purification of the lithium extraction slag. According to the method, the graphite in the waste lithium iron phosphate battery positive and negative electrode mixture lithium extraction slag can be subjected to resourceful treatment, resources can be effectively utilized, and the environment can be effectively protected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solid waste resource recovery, and in particular to a method for purifying graphite in lithium-extracting slag from positive and negative electrode mixtures of waste lithium iron phosphate batteries. Background Art

[0002] At present, researchers at home and abroad are mainly concerned with the recovery of valuable metals in discarded lithium-ion batteries, but pay less attention to the recovery and reuse of electrolytes and negative electrode materials, and the relevant recovery technology is immature. Waste negative electrode materials are usually treated by burning, stockpiling or as steelmaking additives, causing environmental pollution and waste of resources. If the waste negative electrode materials can be recycled and reused to realize the closed-loop cycle of lithium-ion batteries, it will be beneficial to the sustainable development of power lithium-ion batteries.

[0003] The graphite content in discarded lithium-ion batteries is between 12% and 21%. Currently, there are two ways to recycle the graphite in the negative electrode of discarded lithium-ion batteries. One is to recycle the discarded graphite into the negative electrode of lithium batteries through wet methods, fire methods, physical separation, etc.; the other is to transform the discarded graphite into other functional materials, for example, transforming the discarded graphite into adsorption materials, graphene materials, etc. However, the premise of these two recycling methods is that the graphite in the negative electrode of discarded lithium-ion batteries needs to be purified. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a method for purifying graphite in lithium slag from positive and negative electrode mixtures of waste lithium iron phosphate batteries with low cost and high purification rate.

[0005] In order to achieve the above object, the technical solution of the present invention is a method for purifying graphite in lithium slag from positive and negative electrode mixture of waste lithium iron phosphate battery, the specific steps are:

[0006] Step 1: drying and crushing the lithium slag from the positive and negative electrode mixture of waste lithium iron phosphate batteries;

[0007] Step 2, washing the lithium extraction slag obtained in step 1 with water and filtering;

[0008] Step 3, placing the filter residue obtained in step 2 in a hydrochloric acid solution for leaching and filtering;

[0009] Step 4, leaching the filter residue obtained in step 3 in a mixed acid consisting of hydrochloric acid, hydrogen peroxide and hydrofluoric acid, filtering, washing and drying;

[0010] Step 5, placing the leaching product obtained in step 4 in a muffle furnace for calcination, and the obtained high-temperature calcination product is graphite purified from lithium extraction slag.

[0011] The preferred technical solution is that in step 1, the drying temperature is 105°C, the time is 2 hours, and the crushing is 4 to 5 times.

[0012] The preferred technical solution is that the specific step of water washing in step 2 is that the mass ratio of ultrapure water to solid volume of lithium extraction slag liquid is 15 mL / g, and magnetic stirring is carried out at room temperature for 1 hour.

[0013] The preferred technical solution is that the specific steps of acid leaching in step three are as follows: the mass ratio of hydrochloric acid to solid volume of lithium extraction slag liquid is 15 mL / g, and the mixture is placed on a constant temperature magnetic stirrer at 40° C. and stirred for 4 hours.

[0014] The preferred technical solution is that the specific steps of step 4 mixed acid leaching are as follows: the solid volume mass ratio of the mixed acid to the lithium extraction slag liquid is 15 mL / g, the volume ratio of hydrochloric acid, hydrogen peroxide and hydrofluoric acid is 27:2:1, and the mixture is placed on a constant temperature magnetic stirrer at 40°C and stirred for 2 hours.

[0015] In the above technical solution, both hydrogen peroxide and hydrofluoric acid are of industrial grade.

[0016] In the preferred technical solution, the calcination temperature in step 5 is 1050° C. and the calcination time is 3 hours.

[0017] In the above technical solution, the protective atmosphere for calcination in step five is nitrogen.

[0018] In the preferred technical solution, the concentration of hydrochloric acid in steps three and four is 5 mol / L.

[0019] The advantages of the present invention are:

[0020] 1. The present invention can process the graphite in the lithium slag extracted from the positive and negative electrode mixture of waste lithium iron phosphate batteries, which can effectively utilize resources and protect the environment;

[0021] 2. The first acid leaching liquid of the present invention has a high metal content, and can also be extracted step by step to maximize resource utilization;

[0022] 3. The present invention can be applied to metal leaching experiments and the regeneration and repair of graphite in batteries, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. The accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0024] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0025] Figure 1 The SEM spectrum of lithium slag extracted from the positive and negative electrode mixture of waste lithium iron phosphate battery;

[0026] Figure 2XRD spectrum of lithium slag extracted from the positive and negative electrode mixture of waste lithium iron phosphate battery;

[0027] Figure 3 XPS spectrum of lithium slag extracted from the positive and negative electrode mixture of waste lithium iron phosphate battery;

[0028] Figure 4 Raman spectrum of lithium slag extracted from the positive and negative electrode mixture of waste lithium iron phosphate battery;

[0029] Figure 5 This is the SEM image of the purified graphite;

[0030] Figure 6 is the PXRD pattern of purified graphite;

[0031] Figure 7 is the XPS spectrum of purified graphite;

[0032] Figure 8 is the Reman spectrum of purified graphite;

[0033] Fig. 9 This is the surface area diagram of the purified graphite;

[0034] Fig.10 The pore volume diagram of purified graphite;

[0035] Fig.11 This is a graph showing magnetic field measurement data for purified graphite. DETAILED DESCRIPTION

[0036] Embodiment: A method for purifying graphite carbon from lithium slag extracted from positive and negative electrode mixtures of waste lithium iron phosphate batteries comprises the following steps:

[0037] Step 1: drying the waste lithium iron phosphate positive and negative electrode mixture lithium slag at 105°C for 2h and crushing it 4-5 times;

[0038] Step 2, accurately weighing the lithium extraction slag, magnetically stirring it with ultrapure water at room temperature for 1 hour, and filtering it, wherein the mass ratio of ultrapure water to lithium extraction slag liquid-solid volume is 15 mL / g;

[0039] Step 3, placing the filter residue obtained in step 2 in a 5 mol / L hydrochloric acid solution, stirring with magnetic force at a constant temperature of 40°C for 4 hours, wherein the mass ratio of hydrochloric acid to solid volume of lithium extraction residue liquid is 15 mL / g, and filtering after leaching;

[0040] Step 4: placing the filter residue obtained in step 3 in a mixed acid composed of 5 mol / L hydrochloric acid, hydrogen peroxide and hydrofluoric acid and stirring at 40°C for 4 hours, wherein the mass ratio of the mixed acid to the solid volume of the lithium extraction residue is 15 mL / g, and the volume ratio of hydrochloric acid, hydrogen peroxide and hydrofluoric acid is 27:2:1. After leaching, filtering, washing and drying;

[0041] Step 5: calcine the leached product obtained in step 4 at 1050° C. for 3 hours in a muffle furnace protected by nitrogen, and the obtained high-temperature calcined product is graphite purified from lithium slag, and the purity of the graphite can reach 99.8%.

[0042] like Figure 1 , 5 By comparison, it can be seen that most of the waste slag phase is spherical particles, and only a few present lamellar structure. After the slag phase is treated, the spherical particles disappear, and lamellar structure materials exist, and the surface of the purified graphite is smooth.

[0043] like Figure 2 , 6 By comparison, it can be seen that the main diffraction peaks in the PXRD spectrum of the waste slag are consistent with those of iron phosphate and graphite, indicating that the main components of the waste slag are iron phosphate and graphite, and it also contains some Ca, Mg minerals and silicates; the purified graphite sample shows a strong graphite characteristic peak (002) at 2θ=26.5°, indicating that the purified graphite still maintains the layered structure of graphite, and its layered structure is not damaged after acid washing and high-temperature treatment.

[0044] like Figure 3 , 7 By comparison, it can be seen from the XPS full spectrum of the waste slag that the main elements contained in the waste slag are Fe, P, C, Na, Mg, Ca, F, etc.; the element type contained in the purified sample is C, and the signals of other elements have basically disappeared, leaving only graphite components.

[0045] like Figure 4 , 8 By comparison, it can be seen that in the Raman spectrum of the waste residue, D (1300cm -1 ) belt and G(1600cm -1 ) band is the characteristic peak of graphite, D band represents the defects of graphite crystal, and G band represents the carbon atom sp 2 Hybridized in-plane stretching vibration, and I D / I G Less than 1, the graphite purity is low, and metal oxides such as Fe-O (500-1000cm -1 ) and PO4 2- Raman peak (around 1060 cm -1 ); In the Raman spectrum of the purified graphite, it can be seen that the D (1300cm-1) band, G (1600cm -1 ) belt and 2D(2650cm -1 ) band is the characteristic peak of graphite, and I D / I GEqual to 0.37, indicating that the disorder of purified graphite is reduced and the degree of graphitization is improved

[0046] like Fig. 9 , Fig.10 It can be seen that the purified graphite was subjected to BET test, and the results are shown in the figure below. It can be seen from the figure that the N2 adsorption-desorption curve of the sample belongs to the standard H3 type hysteresis loop, and the Langmuir specific surface area of ​​the sample is 5.940m 2 / g, BET specific surface area is 4.803m 2 / g, pore volume 0.003cc / g

[0047] like Fig.11 It can be seen that the magnetic susceptibility of the purified graphite was measured in the magnetic field range of -80 to 80 kOe at 300 K using AC magnetic susceptibility, but no obvious magnetic signal was observed.

[0048] The graphite purified in this embodiment has a high content and good quality, can be recycled and reused in the negative electrode of lithium batteries or converted into adsorption materials, graphene materials, etc., and has good application prospects.

Claims

1. A method for purifying graphite from lithium slag extracted from positive and negative electrode mixtures of waste lithium iron phosphate batteries, characterized in that: The specific steps are: Step 1: drying and crushing the lithium slag from the positive and negative electrode mixture of waste lithium iron phosphate batteries; Step 2, washing the lithium extraction slag obtained in step 1 with water and filtering; Step 3, placing the filter residue obtained in step 2 in a hydrochloric acid solution for leaching and filtering; Step 4, leaching the filter residue obtained in step 3 in a mixed acid consisting of hydrochloric acid, hydrogen peroxide and hydrofluoric acid, filtering, washing and drying; Step 5, placing the leaching product obtained in step 4 in a muffle furnace for calcination, and the obtained high-temperature calcination product is graphite purified from lithium extraction slag.

2. The method for purifying graphite in lithium slag from positive and negative electrode mixture of waste lithium iron phosphate battery according to claim 1, characterized in that: In step 1, the drying temperature is 105°C, the time is 2 hours, and the crushing times are 4 to 5 times.

3. The method for purifying graphite in lithium slag from positive and negative electrode mixture of waste lithium iron phosphate battery according to claim 1, characterized in that: The conditions for water washing in step 2 are that the mass ratio of ultrapure water to solid volume of lithium extraction slag liquid is 15 mL / g, and magnetic stirring is performed at room temperature for 1 hour.

4. The method for purifying graphite in lithium slag from positive and negative electrode mixture of waste lithium iron phosphate battery according to claim 1, characterized in that: The acid leaching conditions in step 3 are as follows: the mass ratio of hydrochloric acid to solid volume of lithium extraction slag is 15 mL / g, and the mixture is placed on a constant temperature magnetic stirrer and stirred at 40° C. for 4 h.

5. The method for purifying graphite in lithium slag from positive and negative electrode mixture of waste lithium iron phosphate battery according to claim 1, characterized in that: The conditions for mixed acid leaching in step 4 are as follows: the mass ratio of the mixed acid to the solid volume of the lithium extraction slag liquid is 15 mL / g, the volume ratio of hydrochloric acid, hydrogen peroxide and hydrofluoric acid is 27:2:1, and the mixture is placed on a constant temperature magnetic stirrer and stirred at 40°C for 2 hours.

6. The method for purifying graphite in lithium slag from positive and negative electrode mixture of waste lithium iron phosphate battery according to claim 1, characterized in that: Step 5: The calcination temperature is 1050°C and the time is 3h.

7. The method for purifying graphite in lithium slag from positive and negative electrode mixture of waste lithium iron phosphate battery according to claim 6, characterized in that: The protective atmosphere for calcination was nitrogen.

8. The method for purifying graphite in lithium slag from positive and negative electrode mixture of waste lithium iron phosphate battery according to claim 4 or 5, characterized in that: The concentration of hydrochloric acid in the calcination steps three and four is 5 mol / L.

Citation Information

Cited By

  • Waste battery material powder, and preparation method therefor and use thereof

    WO2026171119A1