High-transmittance glass capable of transmitting medium-wave ultraviolet rays and glass product
By adjusting the component content in the glass, high transmittance mid-wave ultraviolet glass is prepared, which solves the problems of insufficient transmittance and poor sealing of mid-wave ultraviolet glass in the existing technology, and realizes high-efficiency, long-life mid-wave ultraviolet glass. UV light.
Patent Information
- Application Number
- CN202410865078.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
It is difficult to provide high-transmittance mid-wave ultraviolet glass with the existing technology, and the mid-wave ultraviolet lamp has insufficient sealing and service life, and there is a phenomenon of slow air leakage.
By adjusting the contents of SiO2, B2O3, BaO, Al2O3, Na2O, K2O and TiO2, a high transmittance medium-wave ultraviolet glass is prepared to ensure that the glass transmittance to medium-wave ultraviolet rays exceeds 80%, and the transmittance of short-wave ultraviolet rays is more than 80%. Less than 10%, and can be well sealed with other types of glass to improve the sealing and service life of the lamp.
The medium-wave ultraviolet glass with high transmittance ensures the high efficiency, good sealing and long service life of the medium-wave ultraviolet lamp, avoids slow air leakage, and reduces the attenuation amplitude.
Smart Images

Figure BDA0004921895080000011 
Figure BDA0004921895080000031 
Figure FDA0004921894940000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a medium-wave ultraviolet transparent glass with high transmittance and a glass product. Background Art
[0002] Ultraviolet radiation B (UVB) is the main spectrum of ultraviolet rays reaching the earth's surface that causes biological effects on the body, with a wavelength of 280 to 320 nm. Studies have shown that ultraviolet rays with a wavelength of 280 to 320 nm can react with the chemical chains of special materials, thereby accelerating the chemical reaction rate of the materials. Therefore, ultraviolet rays are often used in light curing and aging experiments.
[0003] Research shows that the higher the intensity of medium-wave ultraviolet rays, the faster the chemical reaction speed, and the higher the production efficiency of the product. In view of this, in order to broaden the application field of medium-wave ultraviolet rays, it is of great significance to develop a medium-wave ultraviolet transparent glass with high transmittance. Summary of the invention
[0004] The technical problem solved by the present invention is to provide a medium-wave ultraviolet transparent glass with high transmittance. The glass provided by the present application has high transmittance to medium-wave ultraviolet rays; and can be well sealed with dumet or other amber glass, and there is no air line on the glass surface. The medium-wave ultraviolet lamp made of it has good energy efficiency, tight sealing, no slow air leakage, and extremely small attenuation.
[0005] In view of this, the present application provides a high-transmittance medium-wave ultraviolet transparent glass, which comprises, by mass percentage:
[0006]
[0007] Preferably, the content of SiO2 is 65-71%.
[0008] Preferably, the content of B2O3 is 1.5-9%.
[0009] Preferably, the content of BaO is 2-8%.
[0010] Preferably, the content of Al2O3 is 1-4%.
[0011] Preferably, the content of Na2O is 4.5-14%; the content of K2O is 8-11%.
[0012] Preferably, the content of TiO2 is 0.1-0.9%.
[0013] Preferably, the glass has a transmittance of >80% for medium-wave ultraviolet rays and a transmittance of <10% for short-wave ultraviolet rays; and an expansion coefficient of (84-94)*10 at 20°C-200°C. -7 .
[0014] The present application also provides a glass product, which is prepared from the high-transmittance medium-wave ultraviolet transparent glass.
[0015] Preferably, the glass product includes a medium-wave ultraviolet transparent glass tube, a medium-wave ultraviolet transparent glass shell, a medium-wave ultraviolet transparent glass sheet, a medium-wave ultraviolet transparent lamp tube, a medium-wave ultraviolet transparent bulb or a medium-wave ultraviolet transparent lamp bead.
[0016] The present application provides a high-transmittance medium-wave ultraviolet transparent glass, which comprises, by mass percentage: SiO2 65-75%, B2O3 1-10%, BaO 1-8%, Al2O3 0.1-5%, Na2O 4-15%, K2O 7-15%, TiO2 0.1~1%; in the glass with high transmittance and medium-wave ultraviolet light, SiO2, as the main body of silicate glass, can form the skeleton of glass, B2O3 can reduce the viscosity of glass and accelerate clarification, BaO fills the network pores of glass, blocks the ion migration channel, is beneficial to improve the resistivity of glass, and also has a fluxing effect, Al2O3 can improve the devitrification of glass, Na2O and K2O can significantly reduce the viscosity of glass and promote the melting of glass, and also determine the expansion coefficient of glass to a large extent, TiO2 can shield short-wave ultraviolet light and adjust the medium-wave peak value; therefore, the glass provided in the present application has a high transmittance of more than 80% for medium-wave ultraviolet light and a transmittance of less than 10% for short-wave ultraviolet light by adding the above components and adjusting the content of the above components, and there is no air line on the surface of the glass, and it can be well sealed with Dumet or other amber glass. The prepared medium-wave ultraviolet lamp (UVB lamp) has high energy efficiency, good sealing, and long service life, and is used for light curing and aging tests. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 A graph showing the wavelength and transmittance of medium-wave ultraviolet light of the 0.99 mm thick glass produced by the present invention;
[0018] Figure 2 The graph is a graph of wavelength and transmittance of medium-wave ultraviolet rays of the 0.68 mm thick glass produced by the present invention. DETAILED DESCRIPTION
[0019] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0020] In view of the high transmittance performance requirements of medium-wave ultraviolet glass in the prior art, the present application provides a medium-wave ultraviolet glass with high transmittance, which is made by adding SiO2, B2O3, BaO, Al2O3, Na2O, K2O and TiO2, and adjusting the content of the above components, so that the obtained silicate glass has a high transmittance of more than 80% for medium-wave ultraviolet rays, and a transmittance of less than 10% for short-wave ultraviolet rays, and there is no air line on the surface of the glass, which can be well sealed with Dumet or other amber glass, and the medium-wave ultraviolet lamp (UVB lamp) prepared has high energy efficiency, good sealing and long service life. Specifically, the embodiment of the present invention discloses a medium-wave ultraviolet glass with high transmittance, which includes, by mass percentage:
[0021]
[0022] In the medium wave ultraviolet transparent glass provided in the present application, the weight content of SiO2 is 65% to 75%. Specifically, the weight content of SiO2 is 65% to 71%. For example, the content of SiO2 is 65%, 65.1%, 65.3%, 65.6%, 66%, 66.4%, 66.9%, 67%, 67.5%, 67.9%, 68%, 68.5%, 68.8%, 69%, 69.3%, 69.4%, 69.7%, 70%, 70.1%, 70.5%, 71%, 71.6%, 71.5%, 72%, 72.1%, 72.8%, 73%, 73.5%, 73.8%, 74%, 74.3%, 74.9% or 75%; it can also be other values within the range. SiO2 is the main body of silicate glass, forming the skeleton of glass in the form of a network of silicon-oxygen tetrahedrons. If the SiO2 content exceeds 75%, the glass will be difficult to melt, and the melting temperature will need to be increased and the melting time will need to be extended, resulting in excessive energy consumption and reduced production efficiency. It will also increase the annealing temperature and softening temperature of the glass and reduce the expansion coefficient. Too little SiO2 will result in poor chemical stability of the glass.
[0023] The content of B2O3 is 1% to 10%, specifically, the content of B2O3 is 1.5 to 9%; for example, the content of B2O3 is 1%, 1.5%, 1.7%, 2%, 2.1%, 2.3%, 3%, 3.1%, 3.2%, 3.5%, 3.7%, 4%, 4.2%, 4.6%, 5%, 5.3%, 5.8%, 6%, 6.3%, 6.7%, 7%, 7.1%, 7.7%, 8%, 8.1%, 8.6%, 9%, 9.1%, 9.3% or 10%, or other values within the range. B2O3 fluxing reduces the viscosity of the glass and accelerates the clarification process; too little B2O3 content has no effect, and too much B2O3 reduces the chemical stability of the glass.
[0024] The medium-wave ultraviolet transparent glass of the present invention contains BaO 1% to 8%, specifically, the content of BaO is 2% to 8%; for example, the content of BaO is 1%, 1.3%, 1.6%, 2%, 2.2%, 2.6%, 3%, 3.1%, 3.5%, 4%, 4.3%, 4.6%, 5%, 5.1%, 5.3%, 6%, 6.2%, 6.9%, 7%, 7.2%, 7.8% or 8%; it can also be other values within the range. Too little BaO content will not work, and too much BaO will make the glass easy to lose transparency. The BaO can fill the network gap of the glass with ions, block the ion migration channel, and increase the resistivity of the glass. It also has a fluxing effect and promotes the melting of the glass. The medium-wave ultraviolet transparent glass of the present invention introduces B2O3 and BaO at the same time, which can also reduce the attenuation amplitude of the glass.
[0025] The content of Al2O3 is 0.1% to 5%, specifically, the content of Al2O3 is 1% to 4%; for example, the content of Al2O3 is 0.1%, 0.5%, 1%, 1.2%, 1.5%, 2%, 2.1%, 2.5%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.5%, 3.8%, 3.9%, 4%, 4.2%, 4.5%, 4.8% or 5.0%, or other values within the range. Al2O3 can significantly improve the devitrification of glass. When Al2O3>5%, the viscosity of the glass melt is too high and glass without bubbles cannot be obtained. If Al2O3<0.1%, the above effect cannot be obtained, and it is difficult to make homogeneous glass and stable molding.
[0026] The content of Na2O in the medium wave ultraviolet transparent glass of the present invention is 4% to 15%, specifically, the content of Na2O is 4.5-14%; for example, the content of Na2O is 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.4%, 8.8%, 9%, 9.4%, 9.7%, 10%, 10.2%, 10.5%, 11%, 11.2%, 11.6%, 12%, 12.3%, 12.5%, 13%, 13.5%, 13.8%, 14%, 14.5%, 14.8% or 15w%; it can also be other values within the range. The content of K2O is 7% to 15%, specifically, the content of K2O is 8% to 11%; for example, the content of K2O is 7%, 7.3%, 8%, 8.5%, 9%, 9.2%, 10%, 10.1%, 10.3%, 10.6%, 10.9%, 11%, 11.1%, 11.6%, 12%, 12.3%, 13%, 13.5%, 14%, 14.6% or 15%; it can also be other values within the range. (Na2O+K2O) 11% to 30%, specifically, (Na2O+K2O) 13% to 22%. Na2O and K2O can significantly reduce the viscosity of glass and promote glass melting. They are good fluxing agents and also largely determine the expansion coefficient of glass. If their content is too little, they will not work and their expansion coefficient will be too low. If their content is too much, the chemical stability of the glass will be reduced. If the content of (Na2O+K2O) exceeds 30%, the expansion coefficient of the glass will reach 94*10 -7 (20℃~200℃) or above, the expansion coefficient does not match that of Dumet and other platinum group glasses, and they cannot be well sealed with the two. During the operation of making medium-wave ultraviolet lamps, they will explode on the spot or have large residual stress, and they will crack and leak during use. The simultaneous introduction of Na2O and K2O has a double alkali effect, which can improve the chemical stability of the glass.
[0027] The content of TiO2 is 0.1-1%, specifically, the content of TiO2 is 0.1%-0.9%; for example, the content of TiO2 is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1.0%; it can also be other values within the range. TiO2 in the present invention mainly plays the role of shielding short-wave ultraviolet rays and adjusting the peak value of medium-wave ultraviolet rays.
[0028] The medium-wave ultraviolet transparent glass provided in the present application also contains a reducing agent or a clarifying agent commonly used in the glass industry.
[0029] In the present application, the method for preparing the medium-wave ultraviolet transparent glass is carried out according to a method well known to those skilled in the art, and the present application does not impose any particular limitation on this method.
[0030] The transmittance of the medium-wave ultraviolet glass provided by the present application is greater than 80%, and the transmittance of the short-wave ultraviolet is less than 10%; the expansion coefficient at 20°C to 200°C is (84 to 94)*10 -7 .
[0031] The present application also provides a glass product, which is prepared from the above-mentioned high-transmittance medium-wave ultraviolet transparent glass.
[0032] Specifically, the glass product may be a medium-wave ultraviolet transparent glass tube, a medium-wave ultraviolet transparent glass shell or a medium-wave ultraviolet transparent glass sheet, or may be a medium-wave ultraviolet transparent lamp, such as a medium-wave ultraviolet transparent lamp tube, a medium-wave ultraviolet transparent bulb or a medium-wave ultraviolet transparent lamp bead.
[0033] In order to further understand the present invention, the high transmittance medium-wave ultraviolet transparent glass provided by the present invention is described in detail below in conjunction with the embodiments, and the protection scope of the present invention is not limited by the following embodiments.
[0034] Example
[0035] Glasses with different specific compositions were prepared according to the components in Table 1, and the properties of the glasses were tested. The results are shown in Table 1.
[0036] Table 1 Data table of glass components in different embodiments
[0037] Glass component (wt%) 1 2 3 4 5 <![CDATA[SiO2]]> 67.5 69.4 68.5 65.1 72.1 <![CDATA[B2O3]]> 2.3 2.1 3.1 3.5 3.2 BaO 5.3 5.1 5.1 6.9 3.1 <![CDATA[Al2O3]]> 2.9 2.8 3.1 3.9 2.1 <![CDATA[Na2O]]> 11.2 9.4 9.7 8.8 8.4 <![CDATA[K2O]]> 10.3 10.6 10.1 11.1 10.9 <![CDATA[TiO2]]> 0.5 0.6 0.4 0.7 0.2 sum 100 100 100 100 100 <![CDATA[Coefficient of expansion: δ * 10 -7 (20 to 200 °C)]]> 88.1 87.2 84.3 84.4 84.1 Transmittance (thickness 0.7mm) wavelength 320nm 82.5 83.5 82.2 85.1 84.1
[0038] A glass with a specific composition is selected from the glasses described in any one of claims 1 to 7 of the present application, and is prepared to have a thickness of 0.99 mm and 0.68 mm, respectively. The wavelength and transmittance curves of the ultraviolet rays are as follows: Figure 1 and Figure 2 shown by Figure 1 It can be seen that the transmittance of glass with a thickness of 0.99 mm for ultraviolet rays with a wavelength of 320 nm is greater than 80%, and can reach 83.8%. The transmittance of glass with a thickness of 0.68 mm for ultraviolet rays with a wavelength of 320 nm is greater than 80%, and can reach 85.0%. This shows that the transmittance of the glass provided in the present application for medium-wave ultraviolet rays can indeed reach more than 80%.
[0039] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0040] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention; to understand how changes in the chemical content of the product affect the expansion coefficient and softening temperature of the product, so that the technicians can have a clearer understanding and mastery of the technology of electronic glass. Various modifications to these embodiments will be obvious to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high transmittance medium-wave ultraviolet transparent glass, characterized in that: In terms of mass percentage, it includes:
2. The glass according to claim 1, characterized in that The content of SiO2 is 65-71%.
3. The glass according to claim 1, characterized in that The content of B2O3 is 1.5-9%.
4. The glass according to claim 1, characterized in that The content of BaO is 2-8%.
5. The glass according to claim 1, characterized in that The content of Al2O3 is 1-4%.
6. The glass according to claim 1, characterized in that The content of Na2O is 4.5-14%; the content of K2O is 8-11%.
7. The glass according to claim 1, characterized in that The content of TiO2 is 0.1-0.9%.
8. The glass according to claim 1, characterized in that The glass has a transmittance of >80% for medium-wave ultraviolet rays and a transmittance of <10% for short-wave ultraviolet rays; and an expansion coefficient of (84-94)*10 at 20°C-200°C. -7 .
9. A glass product prepared from the medium-wave ultraviolet-transmitting glass with high transmittance according to any one of claims 1 to 8.
10. The glass product according to claim 9, characterized in that The glass product comprises a medium-wave ultraviolet transparent glass tube, a medium-wave ultraviolet transparent glass shell, a medium-wave ultraviolet transparent glass sheet, a medium-wave ultraviolet transparent lamp tube, a medium-wave ultraviolet transparent bulb or a medium-wave ultraviolet transparent lamp bead.