Method for reducing thickness of melting material skin of boron-containing aluminosilicate glass
By adding compound modifiers such as Glauber's salt and carbon powder to the glass batch, it promotes the silicate reaction and accelerates the melting of B2O3. This solves the problem of the thickness of the material layer in the electronic glass and improves the clarity and B2O3 uniformity of the finished glass. , suitable for large-scale float glass production.
Patent Information
- Application Number
- CN202411216650.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-09-02
AI Technical Summary
In the production of electronic glass, the use of B2O3 leads to an increase in the thickness of the skin layer, which affects the stability of the production process and the quality of the glass. It is difficult to effectively reduce the thickness of the skin layer with existing technology, especially in the lack of suitable methods in large-scale float glass production lines.
By equipping Glauber's salt, carbon powder, water glass and water to form a composite modifier, add it to the glass batch material for stirring and mixing, and preheat and raise the temperature in the quartz crucible to promote the silicate reaction, accelerate the melting of B2O3, and form a glass liquid. Use a high-temperature video observation device to record clarity and skin thickness.
It effectively reduces the thickness of the material layer, improves the clarity of the finished glass and the uniformity of B2O3 components, and reduces the volatilization of B2O3 during the melting process. It is suitable for large float glass production lines without the need to modify the production line.
Smart Images

Figure CN118851565A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass production, in particular to a method for reducing the thickness of a boron-aluminosilicate glass melting material skin and a boron-aluminosilicate glass melting method. Background Art
[0002] At present, with the development of electronic glass, electronic glass manufacturers have upgraded and optimized the glass formula in order to obtain better glass scratch resistance and drop resistance. All companies have gradually increased the amount of B2O3, that is, boron oxide, in the formula with the use of alkali metals and alkaline earth metals. However, there are also some problems with the use of B2O3. The use of B2O3 will cause aluminosilicate glass to have a more obvious skin layer like borosilicate glass. The existence of the skin layer will cause the production process stability to deteriorate and the apparent quality of the glass to deteriorate, such as the formation of glass tendons, local crystallization, etc., causing the glass composition to change significantly, or the B2O3 content to be significantly lower than the design value and other adverse consequences. At present, the B2O3 content in borosilicate glass is generally above 1.5%. The main function of B2O3 is to reduce the viscosity of the glass at high temperatures, which is conducive to melting and clarification; at low temperatures, it makes the structure tend to be compact and the strength of the product is improved.
[0003] At present, there are generally two ways to deal with the skin layer of the material in production. One is to provide overflow capacity when designing the production line, similar to the B2O3-containing glass fiber industry, and regularly clean up the surface skin by overflow, and use bottom material collection and other methods to avoid entering the molding section; the other is to use a platinum channel to fill the channel with glass liquid, and use precise temperature control and high-temperature melting technology to melt the skin. These two methods have their own advantages and disadvantages. The overflow method is mainly used in the glass fiber industry and is not suitable for use in float production lines; the glass gold channel is generally used in production lines below 80t / d. If used in float glass production lines, the structure in the production line needs to be modified on a large scale, which is costly and difficult to manage. Therefore, it is necessary to provide a method that is suitable for large-scale float glass production lines and does not require the production line to be modified, and can effectively reduce the thickness of the skin in the melting of boron-aluminosilicate glass. Summary of the invention
[0004] The present invention provides a method for reducing the skin thickness of boron-aluminosilicate glass melt to solve the problems raised in the above background technology.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for reducing the skin thickness of boron-containing aluminosilicate glass during melting, characterized in that it comprises the following steps:
[0007] 1) SiO2, Al2O3, Na2O, K2O, MgO, CaO, B2O3, ZrO2, configure the above materials in a certain proportion to form a glass batch;
[0008] 2) Prepare a composite improver by mixing Glauber's salt, carbon powder, water glass and water in a certain proportion;
[0009] 3) Adding a composite improver into the glass batch material and stirring and mixing them fully to form an improved batch material;
[0010] 4) Preheating is performed in a quartz crucible. After preheating to a certain temperature, the improved batch is placed in the quartz crucible, and the quartz crucible is gradually heated at a certain heating rate. The composite improver accelerates the silicate reaction of the improved batch and accelerates the melting of B2O3 until it is heated to a predetermined insulation temperature. The insulation temperature is maintained for a certain period of time to melt the improved batch to form glass liquid.
[0011] Preferably, in the step 1), the ratio of each material in the glass batch is SiO2: 68.5wt%; Al2O3: 8wt%; Na2O: 7wt%; K2O: 1.5wt%; MgO: 7wt%; CaO: 3wt%; B2O3: 4wt%; ZrO2: 0.5wt%.
[0012] Preferably, in the step 2), the proportions of the materials in the composite improver are: 1%-5% of sodium sulfate, 1%-4% of carbon powder, 1%-8% of water glass, and 1.5%-7% of water.
[0013] Preferably, in the step 2), a portion of the improved batch is extracted and kept at 1500°C-1600°C for 5h-6h to form a glass liquid, and the glass liquid is cooled to form a glass block, the glass block is dissolved, and the B2O3 content in the glass is detected.
[0014] Preferably, in the step 4), the quartz crucible is a transparent quartz crucible.
[0015] Preferably, in the step 4), the preheating temperature of the quartz crucible is 1000°C-1100°C, and the heating rate after the improved batch material is put into the quartz crucible is to increase the temperature to 1500°C-1600°C at a rate of 5°C / min, the insulation temperature is 1500°C-1600°C, and the insulation time is 120min-130min.
[0016] The quartz crucible is provided with a high-temperature video observation device for heating and timed shooting and recording. During the heating and insulation process, the high-temperature video observation device is used to shoot and record the clarity of the glass liquid and the thickness of the material skin in different heating time periods of the glass liquid.
[0017] A method for detecting the B2O3 content in glass, which is formed by the above-mentioned method of reducing the thickness of the boron-aluminosilicate glass melting material skin.
[0018] The above-mentioned high-temperature video observation device includes a heating furnace and an observation box. The quartz crucible is placed in the heating furnace. A camera is provided in the observation box. A controller is provided on the top of the observation box. An observation port is provided on one side of the observation box. A corundum tube connected to the interior of the heating furnace is provided on one side of the heating furnace. The port of the corundum tube faces the observation port, and the camera takes pictures of the interior of the heating furnace through the observation port and the corundum tube. The camera is electrically connected to the controller.
[0019] Preferably, a filter is provided at the observation port. The filter is used to help the camera device to insulate heat and prevent the high temperature in the heating furnace from damaging the camera device. The quartz crucible is a rectangular transparent crucible with a hollow interior and an opening at the top. Multiple quartz crucibles can be placed in the heating furnace in a side-by-side arrangement, so that the camera device can simultaneously shoot and compare multiple quartz crucibles.
[0020] The above method is also a boroaluminosilicate glass melting method.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The method for reducing the thickness of the molten material skin of boron-aluminosilicate glass of the present invention comprises the following steps: preparing sodium sulfate, carbon powder, water glass and water to form a composite improver, and adding the composite improver into a glass batch material so that the composite improver accelerates the silicate reaction of the improved batch material, accelerates the melting of B2O3, effectively reduces the thickness of the material skin layer, improves the uniformity of the B2O3-containing component of the glass, and improves the clarity of the glass after forming. The preparation materials of the composite improver are all commonly used materials in chemical production, and the preparation can be completed by directly adding the composite improver into the glass batch material for stirring. The raw material cost is low, and there is no need to modify the production line. The composite improver can be applied to the float process of mass-produced glass, and the raw material ratio of the composite improver can be adjusted accordingly according to the production of glass with different raw material components, and the adaptability is strong. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a comparison diagram of sample 2 and the comparative example taken using a high-temperature visual observation device of the present invention;
[0024] Figure 2 It is a structural schematic diagram of the high temperature video observation device of the present invention;
[0025] 1. Heating furnace; 2. Observation box; 3. Corundum tube; 4. Controller; 5. Observation port. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Reference Figure 1-2 A method for reducing the thickness of a boron-aluminosilicate glass melt comprises the following steps:
[0028] 1) SiO2, Al2O3, Na2O, K2O, MgO, CaO, B2O3, ZrO2, configure the above materials in a certain proportion to form a glass batch;
[0029] 2) Prepare a composite improver by mixing Glauber's salt, carbon powder, water glass and water in a certain proportion;
[0030] 3) Adding a composite improver into the glass batch material and stirring and mixing them fully to form an improved batch material;
[0031] 4) Preheating is performed in a quartz crucible. After preheating to a certain temperature, the improved batch is placed in the quartz crucible, and the quartz crucible is gradually heated at a certain heating rate. The composite improver accelerates the silicate reaction of the improved batch and accelerates the melting of B2O3 until it is heated to a predetermined insulation temperature. The insulation temperature is maintained for a certain period of time to melt the improved batch to form glass liquid.
[0032] In the step 2, the proportions of the materials in the composite improver are: 1%-5% of Glauber's salt, 1%-4% of carbon powder, 1%-8% of water glass, and 1.5%-7% of water.
[0033] In the step 2, a portion of the improved batch is extracted and kept at 1500°C-1600°C for 5h-6h to form a glass liquid. The glass liquid is cooled to form a glass block, the glass block is dissolved, and the B2O3 content in the glass is detected.
[0034] In step 4, the quartz crucible is a transparent quartz crucible.
[0035] In the step 4, the preheating temperature of the quartz crucible is 1000°C-1100°C, and the heating rate after the improved batch material is put into the quartz crucible is to increase the temperature to 1500°C-1600°C at a rate of 5°C / min, the insulation temperature is 1500°C-1600°C, and the insulation time is 120min-130min.
[0036] The quartz crucible is provided with a high-temperature video observation device for heating and timed shooting and recording. During the heating and insulation process, the high-temperature video observation device is used to shoot and record the clarity of the glass liquid and the thickness of the material skin in different heating time periods of the glass liquid.
[0037] A method for detecting the B2O3 content in glass, which is formed by the above-mentioned method of reducing the thickness of the boron-aluminosilicate glass melting material skin.
[0038] Further as follows:
[0039] In the step 1, the ratio of each material in the glass batch is SiO2: 68.5wt%; Al2O3: 8wt%; Na2O: 7wt%; K2O: 1.5wt%; MgO: 7wt%; CaO: 3wt%; B2O3: 4wt%; ZrO2: 0.5wt%.
[0040] The same glass batch material ratio is used, and the materials in the composite improver in step 2 are mixed in different ratios. The test results are as follows:
[0041]
[0042] In the above list, samples 1 to 4 were tested in a certain proportion, samples 5 to 8 were tested by subtracting the composite improver of Glauber's salt, carbon powder, water glass, and water in turn, and the comparative sample was tested without adding the composite improver;
[0043] It can be seen from the above table that after the composite improver of the present invention is prepared in different ratios and reacted with the glass liquid, its skin thickness and B2O3 performance are better than the glass liquid without adding the composite improver. Among them, samples 1 to 4 are all materials and are tested with composite improvers in different ratios. Their skin thickness and B2O3 content are significantly better than the control example. The skin thickness and B2O3 content of tests 5 to 8 are still better than the control example. It can be seen that the composite improver of the present invention can effectively reduce the thickness of the glass melting skin while ensuring the B2O3 content and reducing the volatilization of B2O3 during the melting process.
[0044] The above-mentioned high-temperature video observation device includes a heating furnace 1 and an observation box 2, the quartz crucible is placed in the heating furnace 1, a camera is provided in the observation box 2, a controller 4 is provided on the top of the observation box 2, an observation port 5 is provided on one side of the observation box 2, and a corundum tube 3 connected to the interior of the heating furnace 1 is provided on one side of the heating furnace 1, the end of the corundum tube 3 faces the observation port 5, and the camera takes pictures of the interior of the heating furnace 1 through the observation port 5 and the corundum tube 3, and the camera is electrically connected to the controller 4.
[0045] The observation port 5 is provided with a filter. The filter is used to help the camera device to perform heat insulation and light filtering to prevent the high temperature in the heating furnace 1 from damaging the camera device. The quartz crucible is a rectangular transparent crucible with a hollow interior and an upper opening. Multiple quartz crucibles can be placed in the heating furnace 1 in a side-by-side arrangement, so that the camera device can simultaneously shoot and compare multiple quartz crucibles.
[0046] A top cover is provided on the top of the heating furnace 1, and the quartz crucible is placed through the top of the heating furnace 1. At the same time, the controller 4 is used to observe whether the camera device can observe the glass liquid in the quartz crucible. An electric rotating table can be provided at the bottom of the heating furnace 1. The quartz crucible is placed on the electric rotating table and rotates automatically, so that the camera device can shoot the quartz crucible at multiple angles in the horizontal direction when shooting.
[0047] The present invention adds a composite improver into the glass batch material, and the composite improver accelerates the silicate reaction of the improved batch material, effectively reduces the thickness of the glass melting material skin, reduces the volatilization of B2O3 during melting, and improves the B2O3 content and uniformity in the glass. At the same time, it can be applied to a large number of float glass production lines without the need to modify the production lines.
[0048] The above method is also a boroaluminosilicate glass melting method.
[0049] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0050] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for reducing the skin thickness of a boron-aluminosilicate glass melt, characterized in that: The steps include: 1) SiO2, Al2O3, Na2O, K2O, MgO, CaO, B2O3, ZrO2, configure the above materials in a certain proportion to form a glass batch; 2) Prepare a composite improver by mixing Glauber's salt, carbon powder, water glass and water in a certain proportion; 3) Adding a composite improver into the glass batch material and stirring and mixing them fully to form an improved batch material; 4) Preheating is performed in a quartz crucible. After preheating to a certain temperature, the improved batch is placed in the quartz crucible, and the quartz crucible is gradually heated at a certain heating rate. The composite improver accelerates the silicate reaction of the improved batch and accelerates the melting of B2O3 until it is heated to a predetermined insulation temperature. The insulation temperature is maintained for a certain period of time to melt the improved batch to form glass liquid.
2. The method for reducing the skin thickness of boron-aluminosilicate glass melt according to claim 1, characterized in that: In the step 2), the proportions of the materials in the composite improver are: 1%-5% of sodium sulfate, 1%-4% of carbon powder, 1%-8% of water glass, and 1.5%-7% of water.
3. The method for reducing the skin thickness of boron-aluminosilicate glass melt according to claim 1, characterized in that: In the step 1), the ratio of each material in the glass batch is SiO2: 68.5wt%; Al2O3: 8wt%; Na2O: 7wt%; K2O: 1.5wt%; MgO: 7wt%; CaO: 3wt%; B2O3: 4wt%; ZrO2: 0.5wt%.
4. The method for reducing the skin thickness of boron-aluminosilicate glass melt according to claim 1, characterized in that: In the step 3), a portion of the improved batch material is extracted and kept at 1500°C-1600°C for 5h-6h to form a glass liquid. The glass liquid is cooled to form a glass block, and then the glass block is melted to detect the B2O3 content in the glass.
5. The method for reducing the skin thickness of boron-aluminosilicate glass melt according to claim 1, characterized in that: In the step 4), the quartz crucible is a transparent quartz crucible.
6. The method for reducing the skin thickness of boron-aluminosilicate glass melt according to claim 1, characterized in that: In the step 4), the preheating temperature of the quartz crucible is 1000°C-1100°C, and the heating rate after the improved batch material is put into the quartz crucible is to increase the temperature to 1500°C-1600°C at a rate of 5°C / min, the insulation temperature is 1500°C-1600°C, and the insulation time is 120min-130min.
7. The method for reducing the skin thickness of boron-aluminosilicate glass melt according to claim 5, characterized in that: The quartz crucible is provided with a high-temperature video observation device for heating and timed shooting and recording. During the heating and insulation process, the high-temperature video observation device is used to shoot and record the clarity of the glass liquid and the thickness of the material skin in different heating time periods of the glass liquid.
8. A method for melting boroaluminosilicate glass, characterized in that: A method for melting boroaluminosilicate glass is formed by the method for reducing the thickness of the boroaluminosilicate glass melting material as described in any one of claims 1 to 6.
9. A method for detecting the content of B2O3 in glass, characterized in that: A method for detecting the B2O3 content formed by the method for reducing the thickness of the boron-aluminosilicate glass melting material described in claim 4.
Citation Information
Patent Citations
High borosilicate glass clarifying agent, and preparation method and application thereof
CN106746595A
Glass batch pre-burning treatment process
CN109824244A
Device and method for visually judging glass melting process
CN113336419A
Batch material and method for preparing lithium-containing high-zirconium aluminum silicon glass by using spodumene and zirconite
CN114835397A
Method for reducing boron volatilization of borosilicate glass
CN114956512A