Negative oxygen ion ceramic surface glaze and manufacturing method thereof
Through the combination of modified resin powder, ore powder, nano oxide powder and negative oxygen ion powder, the negative oxygen ion release amount and stability of the ceramic surface glaze are improved, and the problem of insufficient release amount of the existing ceramic glaze is solved. Achieving better air purification and health promotion effects.
Patent Information
- Application Number
- CN202410890079.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-04
AI Technical Summary
On the premise of ensuring performance, it is difficult for existing ceramic glazes to increase the amount of negative oxygen ions released, which affects their effects of purifying the air, eliminating fatigue and promoting health.
Using raw materials such as modified resin powder, ore powder, nano-oxide powder and negative oxygen ion powder, through specific mixing and stirring processes, a ceramic surface glaze with high dispersion and mechanical strength can be prepared to increase the release of negative oxygen ions. .
It improves the negative oxygen ion release and stability of the ceramic surface glaze, while maintaining good wear resistance, adhesion and hardness, and is aldehyde-free and harmless.
Smart Images

Figure BDA0004927216360000041 
Figure BDA0004927216360000051 
Figure BDA0004927216360000061
Abstract
Description
Technical Field
[0001] The invention relates to the field of glazes, and in particular to a negative oxygen ion ceramic surface glaze and a manufacturing method thereof. Background Art
[0002] Ceramic products have become the object of choice for customers with their advantages of high density, good thermal stability, small shrinkage and deformation, easy to wash and keep clean, stable chemical properties, and durability, and have a broad market. In order to enable negative oxygen ion ceramics to release negative ions, the essence is to release electrons. After the released electrons are captured by molecules such as oxygen, "negative oxygen ions" are formed. Negatively charged oxygen molecules can combine with one or several water molecules to form "air negative oxygen ions". When the concentration of negative oxygen ions in the air is greatly increased, negative oxygen ions can neutralize the positively charged groups produced by human metabolism. Therefore, entering it can make people feel very comfortable, as if they have entered a forest. Especially when the humidity in the air increases, the feeling will be more obvious. Natural, odorless, non-toxic, and safe; it has the functions of purifying the air, eliminating human fatigue, and promoting human health; it has antibacterial, sterilization, and deodorization functions. The amount of negative oxygen ions released by ceramic surface glaze has become one of the evaluation indicators of the performance of glaze. The various advantages of existing ceramic glazes have become the key to improving the release of ceramic negative oxygen ions while ensuring that the performance advantages remain unchanged. To this end, the present invention proposes a negative oxygen ion ceramic surface glaze and a manufacturing method thereof to solve the defects and shortcomings of the prior art. Summary of the invention
[0003] In view of the above problems, the present invention provides a negative oxygen ion ceramic surface glaze and a manufacturing method thereof.
[0004] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:
[0005] Preferably, the surface glaze is prepared from the following raw materials in parts by weight:
[0006] 50-90 parts of modified resin powder;
[0007] 20-35 parts of ore powder;
[0008] 10-30 parts of nano oxide powder;
[0009] 10-20 parts of negative oxygen ion powder;
[0010] 20-45 parts of organic solvent:
[0011] Dispersant 0.2-1 part;
[0012] Defoaming agent 0.1-0.5 parts;
[0013] Film-forming aid 0.1-1 part;
[0014] Ultraviolet absorber 0.1-1 part;
[0015] 0.1-0.5 parts of leveling agent.
[0016] Preferably, the surface glaze is prepared from the following raw materials in parts by weight: 60-80 parts of modified resin powder;
[0017] 25-30 parts of ore powder;
[0018] 15-25 parts of nano oxide powder;
[0019] 12-28 parts of negative oxygen ion powder;
[0020] 25-40 parts of organic solvent;
[0021] Dispersant 0.4-0.8 parts;
[0022] Defoaming agent 0.2-0.4 parts;
[0023] Film-forming aid 0.3-0.8 parts;
[0024] 0.3-0.8 parts of ultraviolet absorber;
[0025] 0.2-0.4 parts of leveling agent.
[0026] Preferably, the surface glaze is prepared from the following raw materials in parts by weight: 70 parts of modified resin powder;
[0027] 27 parts of ore powder;
[0028] 20 parts of nano oxide powder;
[0029] 20 portions of negative oxygen ion powder;
[0030] 32 parts of organic solvent:
[0031] 0.6 parts of dispersant;
[0032] 0.3 parts of defoaming agent;
[0033] 0.5 parts of film-forming aid;
[0034] 0.5 parts of ultraviolet absorber;
[0035] 0.3 parts of leveling agent.
[0036] Preferably, the ore powder is made by mixing mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder, and the mass ratio of the mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder is 1:1:1:3.
[0037] Preferably, the negative oxygen ion powder includes tourmaline powder, monazite powder and glacial stone powder, and the mass ratio of the tourmaline powder, monazite powder and glacial stone powder is (1-3):1:1.
[0038] Preferably, the nano oxide powder comprises silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide, and the mass ratio of silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide is 3:2:1:1.
[0039] Preferably, the preparation method specifically comprises the following steps:
[0040] (1) first preparing a modified resin, mixing and dissolving the prepared modified resin with ore powder, nano oxide powder, and negative oxygen ion powder in an organic solvent, and controlling the temperature during dissolution to be 150-200° C., mixing and stirring in a high-speed stirrer at 1500-1600 rpm, and applying an ultrasonic treatment with a power of 100 W throughout the process;
[0041] (2) Add a dispersant, a defoaming agent, a film-forming aid, and an ultraviolet absorber, and disperse them by high-speed stirring to obtain a glaze.
[0042] Preferably, the preparation step of the modified resin powder comprises the following steps:
[0043] (1) mixing and dissolving bisphenol A epoxy resin powder with a molecular weight of 5000-8000 and polyether polyurethane oligomer with terminal isocyanate in tetrahydrofuran solution, and controlling the temperature in the reaction kettle to 210-225° C. and the pressure to 1.35-1.55 MPa;
[0044] (2) Then, a curing agent is added and mixed, and infrasonic and ultrasonic treatments are applied during the reaction process. After solidification, the product is taken out, crushed and sieved to obtain a modified resin powder.
[0045] Preferably, the mass ratio of the epoxy resin to the polyether polyurethane oligomer terminated with isocyanate is (2-5):1.
[0046] Preferably, the mass ratio of the epoxy resin to the polyether polyurethane oligomer terminated with isocyanate is 3:1.
[0047] Due to the adoption of the above-mentioned technical scheme, the beneficial effects of the present invention are as follows: the ceramic surface glaze of the present invention has good wear resistance, adhesion and hardness, and the glaze prepared by the modified resin not only increases the dispersibility of negative oxygen ion powder, nano oxide powder, etc. among the resins, and improves the overall mechanical strength of the resin, but also enables the glaze to have a higher negative oxygen ion release, stable release, and is formaldehyde-free and harmless. DETAILED DESCRIPTION
[0048] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Embodiment 1:
[0050] The raw materials for preparing the negative oxygen ion ceramic surface glaze in this embodiment are as follows:
[0051]
[0052] in:
[0053] The mass ratio of mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder is 1:1:1:3.
[0054] The mass ratio of tourmaline powder, monazite powder and argonite powder is 2:1:1.
[0055] The mass ratio of silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide is 3:2:1:1.
[0056] The method for preparing the negative oxygen ion ceramic surface glaze in this embodiment specifically comprises the following steps:
[0057] (1) first preparing a modified resin, mixing and dissolving a bisphenol A type epoxy resin powder with a molecular weight of 6000 and a polyether polyurethane oligomer with an isocyanate terminal in a tetrahydrofuran solution, ensuring that the mass ratio of the epoxy resin to the polyether polyurethane oligomer with an isocyanate terminal is 3:1, then controlling the temperature in the reactor to 215° C. and the pressure to 1.4 MPa, then adding a curing agent and mixing, applying infrasonic and ultrasonic treatments during the reaction process, taking out after solidification, crushing and sieving, and obtaining a modified resin powder;
[0058] (2) mixing and dissolving the modified resin powder, the ore powder, the nano oxide powder and the negative oxygen ion powder in an organic solvent, controlling the temperature during dissolution at 165° C., mixing and stirring in a high-speed stirrer at 1500 rpm, and applying an ultrasonic treatment with a power of 100 W throughout the process;
[0059] (3) Add a dispersant, a defoaming agent, a film-forming aid, and an ultraviolet absorber, and disperse them by high-speed stirring to obtain a glaze.
[0060] Embodiment 2:
[0061] The raw materials for preparing the negative oxygen ion ceramic surface glaze in this embodiment are as follows:
[0062]
[0063] in:
[0064] The mass ratio of mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder is 1:1:1:3.
[0065] The mass ratio of tourmaline powder, monazite powder and argonite powder is 2:1:1.
[0066] The mass ratio of silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide is 3:2:1:1.
[0067] The method for preparing the negative oxygen ion ceramic surface glaze in this embodiment specifically comprises the following steps:
[0068] (1) first preparing a modified resin, mixing and dissolving bisphenol A type epoxy resin powder with a molecular weight of 5000-8000 and a polyether polyurethane oligomer with an isocyanate terminal in a tetrahydrofuran solution, ensuring that the mass ratio of the epoxy resin to the polyether polyurethane oligomer with an isocyanate terminal is 3:1, then controlling the temperature in the reactor to 220° C. and the pressure to 1.45 MPa, then adding a curing agent and mixing, applying infrasonic and ultrasonic treatments during the reaction process, taking out after solidification, crushing and sieving, and obtaining a modified resin powder;
[0069] (2) mixing and dissolving the modified resin powder, the ore powder, the nano oxide powder and the negative oxygen ion powder in an organic solvent, and controlling the temperature during the dissolution to be 170° C., mixing and stirring in a high-speed stirrer at 1600 rpm, and applying an ultrasonic treatment with a power of 100 W throughout the process;
[0070] (3) Add a dispersant, a defoaming agent, a film-forming aid, and an ultraviolet absorber, and disperse them by high-speed stirring to obtain a glaze.
[0071] Embodiment 3:
[0072] The raw materials for preparing the negative oxygen ion ceramic surface glaze in this embodiment are as follows:
[0073]
[0074] in:
[0075] The mass ratio of mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder is 1:1:1:3.
[0076] The mass ratio of tourmaline powder, monazite powder and argonite powder is 2:1:1.
[0077] The mass ratio of silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide is 3:2:1:1.
[0078] The method for preparing the negative oxygen ion ceramic surface glaze in this embodiment specifically comprises the following steps:
[0079] (1) first preparing a modified resin, mixing and dissolving bisphenol A type epoxy resin powder with a molecular weight of 5000-8000 and a polyether polyurethane oligomer with an isocyanate terminal in a tetrahydrofuran solution, ensuring that the mass ratio of the epoxy resin to the polyether polyurethane oligomer with an isocyanate terminal is 4:1, then controlling the temperature in the reactor to 225° C. and the pressure to 1.55 MPa, then adding a curing agent and mixing, applying infrasonic and ultrasonic treatments during the reaction process, taking out after solidification, crushing and sieving, and obtaining a modified resin powder;
[0080] (2) mixing and dissolving the modified resin powder, the ore powder, the nano oxide powder and the negative oxygen ion powder in an organic solvent, and controlling the temperature during the dissolution to be 200° C., mixing and stirring in a high-speed stirrer at 1500 rpm, and applying an ultrasonic treatment with a power of 100 W throughout the process;
[0081] (3) Add a dispersant, a defoaming agent, a film-forming aid, and an ultraviolet absorber, and disperse them by high-speed stirring to obtain a glaze.
[0082] Embodiment 4:
[0083] The raw materials for preparing the negative oxygen ion ceramic surface glaze in this embodiment are as follows:
[0084]
[0085] in:
[0086] The mass ratio of mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder is 1:1:1:3.
[0087] The mass ratio of tourmaline powder, monazite powder and argonite powder is 3:1:1.
[0088] The mass ratio of silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide is 3:2:1:1.
[0089] The method for preparing the negative oxygen ion ceramic surface glaze in this embodiment specifically comprises the following steps:
[0090] (1) first preparing a modified resin, mixing and dissolving bisphenol A type epoxy resin powder with a molecular weight of 5000-8000 and a polyether polyurethane oligomer with an isocyanate terminal in a tetrahydrofuran solution, ensuring that the mass ratio of the epoxy resin to the polyether polyurethane oligomer with an isocyanate terminal is 5:1, then controlling the temperature in the reactor to 210° C. and the pressure to 1.35 MPa, then adding a curing agent and mixing, applying infrasonic and ultrasonic treatments during the reaction process, taking out after solidification, crushing and sieving, and obtaining a modified resin powder;
[0091] (2) mixing and dissolving the modified resin powder, the ore powder, the nano oxide powder and the negative oxygen ion powder in an organic solvent, and controlling the temperature during the dissolution to be 200° C., mixing and stirring in a high-speed stirrer at 1500 rpm, and applying an ultrasonic treatment with a power of 100 W throughout the process;
[0092] (3) Add a dispersant, a defoaming agent, a film-forming aid, and an ultraviolet absorber, and disperse them by high-speed stirring to obtain a glaze.
[0093] Embodiment 5:
[0094] The raw materials for preparing the negative oxygen ion ceramic surface glaze in this embodiment are as follows:
[0095]
[0096] in:
[0097] The mass ratio of mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder is 1:1:1:3.
[0098] The mass ratio of tourmaline powder, monazite powder and argonite powder is 1:1:1.
[0099] The mass ratio of silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide is 3:2:1:1.
[0100] The method for preparing the negative oxygen ion ceramic surface glaze in this embodiment specifically comprises the following steps:
[0101] (1) first preparing a modified resin, mixing and dissolving bisphenol A type epoxy resin powder with a molecular weight of 5000-8000 and a polyether polyurethane oligomer with an isocyanate terminal in a tetrahydrofuran solution, ensuring that the mass ratio of the epoxy resin to the polyether polyurethane oligomer with an isocyanate terminal is 5:2, then controlling the temperature in the reactor to 215° C. and the pressure to 1.45 MPa, then adding a curing agent and mixing, applying infrasonic and ultrasonic treatments during the reaction process, taking out after solidification, crushing and sieving, and obtaining a modified resin powder;
[0102] (2) mixing and dissolving the modified resin powder, the ore powder, the nano oxide powder and the negative oxygen ion powder in an organic solvent, and controlling the temperature during the dissolution to be 185° C., mixing and stirring in a high-speed stirrer at 1500 rpm, and applying an ultrasonic treatment with a power of 100 W throughout the process;
[0103] (3) Add a dispersant, a defoaming agent, a film-forming aid, and an ultraviolet absorber, and disperse them by high-speed stirring to obtain a glaze.
[0104] Comparative Example 1:
[0105] The raw materials and preparation steps for preparing the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, except for the step of preparing the modified resin, which is specifically as follows:
[0106] Preparation of modified resin powder:
[0107] (1) firstly, bisphenol A type epoxy resin powder with a molecular weight of 6000 and polyether polyurethane oligomer with an isocyanate terminal are mixed and dissolved in a tetrahydrofuran solution, and the mass ratio of the epoxy resin to the polyether polyurethane oligomer with an isocyanate terminal is ensured to be 1:1;
[0108] (2) Then, the temperature in the reactor is controlled to be 215° C. and the pressure is 1.45 MPa, and then a curing agent is added and mixed. During the reaction, infrasonic and ultrasonic treatments are applied. After solidification, the product is taken out, crushed and sieved to obtain a modified resin powder.
[0109] Comparative Example 2:
[0110] The raw materials and preparation steps for preparing the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, except for the step of preparing the modified resin, which is specifically as follows:
[0111] Preparation of modified resin powder:
[0112] (1) firstly, bisphenol A type epoxy resin powder with a molecular weight of 6000 and polyether polyurethane oligomer with terminal isocyanate are mixed and dissolved in tetrahydrofuran solution, and the mass ratio of epoxy resin to polyether polyurethane oligomer with terminal isocyanate is ensured to be 2:1;
[0113] (2) Then, the temperature in the reactor is controlled to be 215° C. and the pressure is 1.45 MPa, and then a curing agent is added and mixed. During the reaction, infrasonic and ultrasonic treatments are applied. After solidification, the product is taken out, crushed and sieved to obtain a modified resin powder.
[0114] Comparative Example 3:
[0115] The raw materials and preparation steps for preparing the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, except for the step of preparing the modified resin, which is specifically as follows:
[0116] Preparation of modified resin powder:
[0117] (1) firstly, bisphenol A type epoxy resin powder with a molecular weight of 6000 and polyether polyurethane oligomer with an isocyanate terminal are mixed and dissolved in a tetrahydrofuran solution, and the mass ratio of the epoxy resin to the polyether polyurethane oligomer with an isocyanate terminal is ensured to be 6:1;
[0118] (2) Then, the temperature in the reactor is controlled to be 215° C. and the pressure is 1.45 MPa, and then a curing agent is added and mixed. During the reaction, infrasonic and ultrasonic treatments are applied. After solidification, the product is taken out, crushed and sieved to obtain a modified resin powder.
[0119] Comparative Example 4:
[0120] The raw materials and preparation steps for preparing the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, except for the step of preparing the modified resin, which is specifically as follows:
[0121] Preparation of modified resin powder:
[0122] (1) firstly, bisphenol A type epoxy resin powder with a molecular weight of 6000 and polyether polyurethane oligomer with an isocyanate terminal are mixed and dissolved in a tetrahydrofuran solution, and the mass ratio of the epoxy resin to the polyether polyurethane oligomer with an isocyanate terminal is ensured to be 7:1;
[0123] (2) Then, the temperature in the reactor is controlled to be 215° C. and the pressure is 1.45 MPa, and then a curing agent is added and mixed. During the reaction, infrasonic and ultrasonic treatments are applied. After solidification, the product is taken out, crushed and sieved to obtain a modified resin powder.
[0124] Comparative Example 5:
[0125] The preparation steps of the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, except that the raw materials are different, specifically: the modified resin is ordinary bisphenol A epoxy resin powder
[0126] Comparative Example 6:
[0127] The steps for preparing the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, except for the difference in raw materials, specifically: the modified resin is ordinary acrylic resin powder.
[0128] Comparative Example 7:
[0129] The preparation steps of the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, wherein: there is no nano-oxide in the raw materials.
[0130] Comparative Example 8:
[0131] The preparation steps of the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, wherein the nano-oxide is silicon dioxide.
[0132] Comparative Example 9:
[0133] The preparation steps of the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, wherein the nano-oxide is titanium dioxide.
[0134] Comparative Example 10:
[0135] The preparation steps of the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, wherein the negative oxygen ion powder is tourmaline powder.
[0136] Comparative Example 11:
[0137] The preparation steps of the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, wherein the negative oxygen ion powder is monazite powder.
[0138] Comparative Example 12:
[0139] The preparation steps of the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, wherein the negative oxygen ion powder is Qibingshi powder.
[0140] Comparative Example 13:
[0141] The preparation steps of the negative oxygen ion ceramic surface glaze in this comparative example are the same as those in Example 1, except that: there is no negative oxygen ion powder.
[0142] Performance testing:
[0143] 1. Detection of negative oxygen ion release of ceramic glaze:
[0144] The prepared glaze is evenly coated on a 3cm×3cm square ceramic sheet, hardened and formed by ultraviolet light, and then placed in a sealed chamber filled with a mixture of heated saturated air and water vapor. The temperature in the sealed chamber is controlled to 30°C and the relative humidity is 95%, so that the glaze on the upper layer of the ceramic sheet releases negative oxygen ions in the sealed chamber. Finally, the amount of negative oxygen ions in the sealed chamber is measured.
[0145] 2. Hardness test of ceramic glaze surface:
[0146] The hardness of the prepared glaze is tested according to the standard GB / T6739-1996, using the A method testing machine method. The larger the H value, the greater the hardness of the glaze layer.
[0147] 3. Test on the wear resistance of ceramic glaze surface
[0148] The ceramic glazes prepared in the above examples and comparative examples were tested for wear resistance according to the existing glazed tile surface wear resistance method (ISO 10545-7:1996 Determination of resistance to surface abrasion for glazed tiles).
[0149] The existing test steps are as follows: the abrasive material uses steel balls with a grade specified in ISO10545-7 and 20 ml of deionized water plus 3.0 g of 80 mesh corundum sand or 3.0 g of 80 mesh quartz sand.
[0150] The test samples of Examples 1-5 and Comparative Examples 1-13 were prepared respectively. The sample preparation method was as follows: glazes of equal mass were coated on ceramic sheets of the same size and cured for the same time to obtain samples. The glaze surface was tested by the above-mentioned tools. The samples prepared in each embodiment were cleaned and dried to constant weight before and after the wear resistance test, and their weights were recorded. The wear results of each embodiment were determined based on the weighing results before and after the test.
[0151] Table 1:
[0152]
[0153] Table 2:
[0154]
[0155] Based on the above, we can conclude that:
[0156] (1) The final hardness of the ceramic surface glaze is different when the mass ratio of epoxy resin and polyether polyurethane oligomer with isocyanate terminal is different. Specifically, when the epoxy resin is higher, the hardness of the ceramic surface glaze is greater, but the release of negative oxygen ions will decrease.
[0157] (2) When the specific gravity of the polyether polyurethane oligomer with an isocyanate terminal in the step of preparing the modified resin is increased, the release amount of negative oxygen ions of the final ceramic surface glaze can be effectively increased, but the hardness of the ceramic surface glaze will also decrease;
[0158] (3) When the specific gravity of the epoxy resin in the step of preparing the modified resin is increased, the wear resistance of the ceramic surface glaze can be effectively improved.
[0159] 4. The adhesion test of glaze shall be carried out in accordance with GB / T9286-1998 "Scratch test of paint and varnish film":
[0160] The test results are classified as follows:
[0161] Level 0: The cutting edge is completely smooth, without any falling off;
[0162] Level 1: A small amount of coating falls off at the intersection of the cuts, but the cross-cut area affected cannot be significantly greater than 5%;
[0163] Level 2: Coating peels off at the intersection of the cuts and / or along the edges of the cuts, and the affected cross-cut area is significantly greater than 5%, but not significantly greater than 15%;
[0164] Level 3: The coating partially or completely falls off in large pieces along the cut edge, and / or partially or completely peels off at different parts of the grid, and the affected cross-cut area is significantly greater than 15%, but not significantly greater than 35%;
[0165] Level 4: The coating peels off in large pieces along the cut edges, and / or some squares are partially or completely peeled off. The affected cross-cut area is significantly greater than 35%, but not significantly greater than 65%;
[0166] Level 5: The degree of thorn drop exceeds that of level 4.
[0167] Table 3:
[0168]
[0169] Table 4:
[0170]
[0171] Based on the above, we can conclude that:
[0172] (1) When silicon dioxide, titanium dioxide, zirconium dioxide, and zinc oxide in nano-oxide powder are reduced or removed, the adhesion and wear resistance of the final ceramic surface glaze are affected;
[0173] (2) When the raw materials of negative oxygen ion powder are changed, such as increasing the content of tourmaline powder, the release of negative oxygen ions can be increased, but the overall adhesion of the glaze on the ceramic surface will be reduced; reducing the content of tourmaline powder can increase the overall adhesion of the glaze on the ceramic surface but will reduce the release of negative oxygen ions on the ceramic surface glaze.
[0174] 4. According to the standards of GB18582-2008 "Limits of Harmful Substances in Interior Wall Paints for Interior Decoration Materials" and JG / T24-2000 "Synthetic Resin Emulsion Sand Wall Architectural Paints", the ceramic glaze prepared in this embodiment is tested:
[0175]
[0176] Table: Hazardous Substance Limit Requirements:
[0177] The data statistics of the ceramic glaze harmful substance limit requirements of test examples 1-5 are as follows:
[0178]
[0179] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
[0180] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A negative oxygen ion ceramic surface glaze, characterized in that: The surface glaze is prepared from the following raw materials in parts by weight: 50-90 parts of modified resin powder; 20-35 parts of ore powder; 10-30 parts of nano oxide powder; 10-20 parts of negative oxygen ion powder; 20-45 parts of organic solvent: Dispersant 0.2-1 part; Defoaming agent 0.1-0.5 parts; Film-forming aid 0.1-1 part; 0.1-1 part of ultraviolet absorber; 0.1-0.5 parts of leveling agent.
2. The negative oxygen ion ceramic surface glaze according to claim 1, characterized in that: The surface glaze is prepared from the following raw materials in parts by weight: 60-80 parts of modified resin powder; 25-30 parts of ore powder; 15-25 parts of nano oxide powder; 12-28 parts of negative oxygen ion powder; 25-40 parts of organic solvent; Dispersant 0.4-0.8 parts; Defoaming agent 0.2-0.4 parts; Film-forming aid 0.3-0.8 parts; 0.3-0.8 parts of ultraviolet absorber; 0.2-0.4 parts of leveling agent.
3. The negative oxygen ion ceramic surface glaze according to claim 1, characterized in that: The surface glaze is prepared from the following raw materials in parts by weight: 70 parts of modified resin powder; 27 parts of ore powder; 20 parts of nano oxide powder; 20 portions of negative oxygen ion powder; 32 parts of organic solvent: 0.6 parts of dispersant; 0.3 parts of defoaming agent; 0.5 parts of film-forming aid; 0.5 parts of ultraviolet absorber; 0.3 parts of leveling agent.
4. The negative oxygen ion ceramic surface glaze according to claim 1, characterized in that: The ore powder is prepared by mixing mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder, and the mass ratio of the mullite powder, potassium feldspar powder, sodium feldspar powder and kaolin powder is 1:1:1:
3.
5. The negative oxygen ion ceramic surface glaze according to claim 1, characterized in that: The negative oxygen ion powder comprises tourmaline powder, monazite powder and glacial stone powder, and the mass ratio of the tourmaline powder, monazite powder and glacial stone powder is (1-3):1:
1.
6. The negative oxygen ion ceramic surface glaze according to claim 1, characterized in that: The nano oxide powder comprises silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide, and the mass ratio of silicon dioxide, titanium dioxide, zirconium dioxide and zinc oxide is 3:2:1:
1.
7. The method for manufacturing the negative oxygen ion ceramic surface glaze according to any one of claims 1 to 6, characterized in that: The preparation method specifically comprises the following steps: (1) first preparing a modified resin, mixing and dissolving the prepared modified resin with ore powder, nano oxide powder, and negative oxygen ion powder in an organic solvent, and controlling the temperature during dissolution to be 150-200° C., mixing and stirring in a high-speed stirrer at 1500-1600 rpm, and applying an ultrasonic treatment with a power of 100 W throughout the process; (2) Add a dispersant, a defoaming agent, a film-forming aid, an ultraviolet absorber and a leveling agent, and disperse them by high-speed stirring to obtain a glaze.
8. The method for manufacturing the negative oxygen ion ceramic surface glaze according to claim 7, characterized in that: The preparation step of the modified resin powder comprises the following steps: (1) mixing and dissolving bisphenol A epoxy resin powder with a molecular weight of 5000-8000 and polyether polyurethane oligomer with terminal isocyanate in tetrahydrofuran solution, and controlling the temperature in the reaction kettle to 210-225° C. and the pressure to 1.35-1.55 MPa; (2) Then, a curing agent is added and mixed, and infrasonic and ultrasonic treatments are applied during the reaction process. After solidification, the product is taken out, crushed and sieved to obtain a modified resin powder.
9. The method for manufacturing the negative oxygen ion ceramic surface glaze according to claim 8, characterized in that: The mass ratio of the epoxy resin to the polyether polyurethane oligomer having an isocyanate terminal is (2-5):
1.
10. The method for manufacturing the negative oxygen ion ceramic surface glaze according to claim 9, characterized in that: The mass ratio of the epoxy resin to the polyether polyurethane oligomer having isocyanate at the end is 3:1.
Citation Information
Patent Citations
Additive capable of releasing negative oxygen ions and preparation method of additive
CN106904979A
Synthetic energy stone and manufacturing method thereof
CN107538624A
Digital glaze with negative ion function, preparation method thereof, and functional ceramic
CN111732447A
Insulating coating composition
CN112094561A
Long-acting antibacterial radiation-proof negative oxygen ion far-infrared coating and preparation method thereof
CN112375445A