Grouting reinforcement material for fractured rock mass and preparation method thereof
By using blast furnace slag instead of cement in the grouting material and combining it with water glass and sodium hydroxide, a new grouting reinforcement material was prepared, which solved the problems of large cement consumption, high energy consumption and low recycling of waste slag, and achieved energy conservation. , waste utilization and performance optimization effects.
Patent Information
- Application Number
- CN202410815844.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-29
AI Technical Summary
The cement used in existing grouting materials in deep mining projects results in high energy consumption, high carbon emissions and low waste residue recycling, making it difficult to meet green and low-carbon goals.
Blast furnace slag was used to replace part of the cement, combined with water glass and sodium hydroxide, to prepare a new grouting reinforcement material, and the water-cement ratio and component ratio were adjusted to optimize fluidity, gelling time and compressive strength.
It effectively reduces the cement consumption of grouting materials, reduces energy consumption and carbon emissions, realizes the effective utilization of waste residue, and improves the fluidity, stability and compressive strength of the material.
Smart Images

Figure CN118851598A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of novel grouting material synthesis, and in particular to a grouting reinforcement material for broken rock mass and a preparation method thereof. Background Art
[0002] With the rapid development of my country's social economy, the demand for mineral resources is also increasing. In order to meet the amount of mineral resources required for engineering construction, my country's shallow mineral resources have gradually become scarce due to the vigorous mining in the early stage. Therefore, the mining of mineral resources has gradually entered the deep mining stage. For deep mining projects, they are often in a complex environment of "three highs and one disturbance", which means that deep mining projects are often carried out under unfavorable geological conditions, and broken rock mass is a common type of unfavorable geological conditions.
[0003] At present, grouting reinforcement technology is one of the main technical means to solve the problem of instability and destruction of broken rock mass in underground engineering. However, the most commonly used cement-based materials in grouting engineering are inorganic grouting materials. It is obvious that the demand for cement in many projects is large, which has led to a huge production of cement in my country in recent years. With the mass production of cement, its raw material energy is also consumed significantly, and a large amount of carbon dioxide is emitted during the production process. Therefore, in order to achieve the goal of green and low-carbon, it is of practical significance to find a suitable material to replace cement to reduce the amount of cement in grouting engineering. The mineral composition and chemical composition of blast furnace slag powder are relatively close to those of cement, and blast furnace slag is an industrial waste slag produced during steel smelting. Its utilization is conducive to energy saving, so blast furnace slag is expected to become a substitute for cement. With the continuous expansion of the market demand for pig iron, the emission of slag has been in a high-yield state, and its annual emission has exceeded 100 million tons. Therefore, the study of replacing part of the cement with blast furnace slag as a mixture in grouting materials has great practical significance in terms of energy saving and waste utilization. Summary of the invention
[0004] The purpose of this application is to propose a grouting reinforcement material for broken rock mass and its preparation method, aiming to use blast furnace slag to replace cement. On the one hand, it can turn industrial waste slag produced during steel smelting into treasure, and on the other hand, it can synthesize a new type of grouting reinforcement material that can replace the traditional pure cement slurry with a water-cement ratio of 0.8.
[0005] On the one hand, the present application proposes a grouting reinforcement material for broken rock mass, wherein the grouting reinforcement material is composed of cement, blast furnace slag, water glass, sodium hydroxide and water.
[0006] In summary, this application proposes a new grouting reinforcement material for broken rock masses, which can effectively reduce the amount of cement in the grouting material, solve the problems of high raw material costs, large industry carbon emissions and low waste residue recycling, and the fluidity, gelation time and compressive strength of the material can be changed according to actual engineering needs by changing the raw material composition ratio to meet the requirements of grouting material performance.
[0007] In some embodiments, the ratio of the blast furnace slag replacing the cement is 10%~50%, the water glass modulus ranges from 1.0~3.0, the alkali concentration range of the grouting reinforcement material is 1%~3%, and the water-cement ratio of the grouting reinforcement material is set to 0.7~0.9.
[0008] In some embodiments, the contents of the components of the grouting reinforcement material are, by mass percentage, 26% to 50% cement, 5% to 30% blast furnace slag, 1.5% to 10% water glass, 0.05% to 1.5% sodium hydroxide, and 35% to 45% water.
[0009] In some embodiments, the cement comprises the following components by mass percentage: SiO2 22%-23%, Al2O3 4%-5%, CaO 62%-63%, MgO 1.5%-2%, Fe2O3 2%-3%, SO3 2.5%-3%, In some embodiments, the blast furnace slag includes the following components by mass percentage: SiO2 33%~34%, Al2O3 15%~16%, CaO 37%~38%, MgO 8%~9%, Fe2O3 0.5%~1%, and TiO2 1.5%~2%.
[0010] In some embodiments, the water glass comprises the following components by mass percentage: SiO2 29%~30%, Na2O 13%~14%, H2O 56%~57%.
[0011] In some embodiments, the Baume degree of the water glass is 50, and the density of the water glass is 1.48 g / cm 3 , the water glass modulus is 2.25.
[0012] In some embodiments, the sodium hydroxide has a purity of at least 96%.
[0013] In some embodiments, the fluidity of the grouting reinforcement material is 334~418mm, the water separation rate is 0.5~4%, the initial setting time is 95~496min, the final setting time is 120~571min, and the compressive strength is 2.24~8.40MPa.
[0014] On the other hand, the present application also proposes a method for preparing a grouting reinforcement material for a broken rock mass, the preparation method comprising: According to the composition ratio of the raw materials, the masses of various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and water and water glass are mixed and stirred; Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0015] Compared with the prior art, this application has the following advantages: 1. Compared with pure cement grouting material, the new grouting reinforcement material proposed in this application has lower cost.
[0016] 2. This application uses industrial waste slag to replace part of the cement when preparing new grouting reinforcement materials, thus turning waste into treasure. That is, industrial waste slag is used as raw material, which can reduce the cement usage by 50% to the greatest extent, and has great practical significance for energy conservation and waste utilization.
[0017] 3. The new grouting reinforcement material proposed in this application has excellent properties such as fluidity, water separation rate, initial setting time, final setting time and compressive strength.
[0018] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become apparent from the following description, or will be understood through the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A schematic diagram of the reaction between water glass and slag according to an example of the present application is shown. DETAILED DESCRIPTION
[0020] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Several embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0022] Reaction mechanism of grouting reinforcement materials in this application: The curing process of water glass-slag-cement composite grouting material is formed by a series of complex physical and chemical reactions of multiple materials. After a series of experimental studies, the reaction mechanism of alkali-activated slag cement-based grouting material can be mainly attributed to the following aspects: 1) Hydration reaction of cement: The hydration reaction of cement mainly includes hydration reactions of tricalcium silicate, dicalcium silicate, tricalcium aluminate, etc. The hydration reaction of tricalcium silicate is the fastest reaction among the cement clinker components, which determines the early strength of cement. Its main hydration products are CSH gel and Ca(OH)2. The reaction process is as shown in formula (1): (1) The hydration process of dicalcium silicate is similar to that of tricalcium silicate, but its hydration rate is slower. It determines the later mechanical properties of cement. The specific reaction is as shown in formula (2): (2) The hydration reaction of tricalcium aluminate is the most rapid reaction among cement clinker components. In pure water, its hydration releases a large amount of heat, which leads to an increase in temperature and an increase in the hydration rate. At room temperature, its hydration product is hydrated calcium aluminate. The reaction formula is as follows: (3) In the presence of gypsum, tricalcium aluminate reacts with gypsum to form ettringite. The reaction process is as shown in formula (4): (4) 2) Reaction of cement and water glass: The water glass solution undergoes a hydrolysis reaction, causing the solution to be in an alkaline environment, generating sodium silicate colloid. The reaction process is shown in formula (5). As the cement hydration reaction proceeds, Ca(OH)2 generated by the hydration of tricalcium silicate and dicalcium silicate reacts with colloidal sodium silicate to generate CSH gel. The specific reaction formula is formula (6). As the reaction proceeds, the Ca(OH)2 in the entire solution is rapidly consumed, causing the equilibrium system of the cement hydration reaction to be continuously destroyed, thereby accelerating the cement hydration reaction rate and reducing the setting time of the entire grouting solution.
[0023] (5) (6) 3) Reaction of slag and water glass: The phase structure of slag glass is divided into calcium-rich phase and silicon-rich phase. The calcium-rich phase tightly wraps the silicon-rich phase. When the slag reacts, the outer calcium-rich phase must be decomposed first. However, in pure aqueous solution, the water molecules are not enough to stimulate and destroy the calcium-rich phase, so the slag and water hardly react. However, in the alkaline activator water glass sodium silicate solution, the water glass hydrolysis makes the entire solution environment alkaline. In a strong alkaline environment, the ions produced by the water glass hydrolysis disintegrate the glass structure of the slag, thereby reacting to form products such as CSH gel. The specific reaction of slag and water glass can be roughly divided into four stages, such as Figure 1 As shown: (I) The sodium silicate solution undergoes a hydrolysis reaction, making the solution alkaline and generating free Na + and OH - , the slag surface reacts; (II) In Na + and OH - Under the stimulation of , the calcium-rich phase of the slag is first decomposed, and the Ca + / Mg + Dissolution, the reaction process is shown in formula (7); (III) When the calcium-rich phase is destroyed and decomposed, Ca + It reacts with silicate ions produced by hydrolysis of water glass to form CSH gel. The reaction process is shown in formula (8); (IV) With Na + and OH - As a result, the silicon-rich phase in the slag glass structure is gradually decomposed and destroyed by free ions, and [SiO4] is dissolved inside. 4- and [AlO4] 5- , and again with the released Ca + The reaction generates CSH gel and hydrotalcite-like phase, and the reaction process is shown in formula (9).
[0024] (7) (8) (9) Embodiment 1 According to the composition ratio of cement 48.96%, slag 5.44%, water glass 1.76%, sodium hydroxide 0.39% and water 43.45%, various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred respectively.
[0025] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0026] Embodiment 2 According to the composition ratio of cement 47.57%, slag 5.29%, water glass 5.13%, sodium hydroxide 0.45% and water 41.56%, various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred respectively.
[0027] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0028] Embodiment 3 According to the composition ratio of cement 45.91%, slag 5.10%, water glass 9.89%, sodium hydroxide 0.22% and water 38.88%, various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred.
[0029] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0030] Embodiment 4 According to the composition ratio of cement 37.30%, slag 15.99%, water glass 3.45%, sodium hydroxide 0.76% and water 42.51%, various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred respectively.
[0031] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0032] Embodiment 5 According to the composition ratio of cement 36.12%, slag 15.48%, water glass 7.51%, sodium hydroxide 0.67% and water 40.22%, various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred respectively.
[0033] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0034] Embodiment 6 According to the component ratio of cement 37.77%, slag 16.19%, water glass 3.49%, sodium hydroxide 0.08% and water 42.48%, the masses of various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred respectively.
[0035] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0036] Embodiment 7 According to the component ratio of cement 26.11%, slag 26.11%, water glass 5.06%, sodium hydroxide 1.12% and water 41.60%, the masses of various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred respectively.
[0037] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0038] Embodiment 8 According to the component ratio of cement 27.09%, slag 27.09%, water glass 2.63%, sodium hydroxide 0.23% and water 42.97%, the masses of various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred respectively.
[0039] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0040] Embodiment 9 According to the composition ratio of cement 26.22%, slag 26.22%, water glass 6.78%, sodium hydroxide 0.15% and water 40.63%, various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and the water and water glass are mixed and stirred respectively.
[0041] Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
[0042] Comparative Example 1 Mix the components of 55.56% cement and 44.44% water, pour into a mixer and mix evenly.
[0043] The chemical composition of the cement used in Examples 1-9 and Comparative Example 1 of the present application is shown in Table 1 below: Table 1 The chemical composition of the slag used in Examples 1-9 of the present application is shown in Table 1 below: Table 2 The water glass used in Examples 1-9 of the present application is sodium water glass, and its molecular formula is Na2O·nSiO2. The specific parameters of the water glass are shown in Table 3 below: Table 3 The sodium hydroxide used in Examples 1-9 of the present application is a white uniform granular solid with a purity of ≥96%.
[0044] Please refer to Table 4 below, which shows the data table of slag replacement rate, water glass modulus, and alkali concentration (the ratio of the mass of Na2O to the sum of the mass of slag and cement) corresponding to the schemes of Examples 1-9 respectively: Table 4 The grouting reinforcement materials obtained in Examples 1-9 and the traditional grouting material obtained in Comparative Example 1 were tested for performance, and the test method was as follows: 1. Fluidity test: First, place the truncated cone mold on a horizontal flat plate, and load the grouting liquids obtained in Examples 1-9 and Comparative Example 1 into the truncated cone mold respectively, and then lift it vertically. After 30 seconds, measure the range of two mutually perpendicular directions where the slurry diffuses the most. Finally, take the average value of the fluidity. Each group of slurry is tested three times.
[0045] 2. Water separation rate test: Take 100 mL of the slurry obtained in Examples 1-9 and Comparative Example 1 and pour them into a 100 mL measuring cylinder; after standing for 2 hours, until the upper layer of water no longer increases, measure the volume of the separated water and calculate the water separation rate.
[0046] 3. Gel time test: Start timing when water is added, then put the grouting slurry obtained in Examples 1-9 and Comparative Example 1 into the test mold, scrape the slurry surface flat, and then put it into the curing box for curing; start measuring after the specimen has been cured for 60 minutes, replace the initial setting test needle according to the Vicat instrument operation requirements and zero the instrument. When the test needle freely falls to 4±1mm from the glass bottom plate, the slurry is in the initial setting state. After the initial setting test is completed, turn the test mold 180° and continue to put it into the curing box for curing. After 15 minutes, perform the first final setting test, replace the Vicat instrument with the final setting test needle, and when the test needle freely falls to no more than 0.5mm from the sample and leaves no obvious traces on the sample surface, the slurry reaches the final setting state.
[0047] 4. The grouting liquids obtained in Examples 1-9 and Comparative Example 1 were respectively placed in standard cylindrical test molds with a diameter of 50 mm and a height of 100 mm. After the specimens were cured for 24 hours, they were demolded and numbered. The demolded specimens were then placed in a curing box for curing. The curing humidity was 90% and the curing temperature was controlled at 20±5°C. After the specimens were cured for 28 days, a uniaxial compressive strength test was performed. Each group of specimens was tested three times, and the final compressive strength was the average value of its peak strength.
[0048] The performance results of the grouting materials of various embodiments and comparative examples measured according to the above steps are shown in Table 5 below: Table 5 As shown in Table 5, the initial setting and final setting time of the optimal group of grouting materials are not much different from those of the control group; in terms of 28-day compressive strength performance, the optimal group is slightly lower than the control group; in terms of fluidity performance, the optimal group is significantly better than the control group; in terms of water separation rate performance, the water separation rate of the optimal group is less than 5% to meet the stability requirements, while the water separation rate of the control group is much higher than the optimal group and does not meet the stability requirements. From the comparison results of the four performance indicators, it can be seen that the alkali-activated slag cement-based grouting material with the optimal mix ratio can replace the pure cement slurry with a water-cement ratio of 0.8 in actual engineering applications.
[0049] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A grouting reinforcement material for broken rock mass, characterized in that: The grouting reinforcement material consists of cement, blast furnace slag, water glass, sodium hydroxide and water.
2. The grouting reinforcement material for broken rock mass according to claim 1, characterized in that: The ratio of the blast furnace slag replacing the cement is 10% to 50%, the water glass modulus ranges from 1.0 to 3.0, the alkali concentration range of the grouting reinforcement material is 1% to 3%, and the water-cement ratio of the grouting reinforcement material is set to 0.7 to 0.
9.
3. The grouting reinforcement material for broken rock mass according to claim 1, characterized in that: Calculated by mass percentage, the contents of the components of the grouting reinforcement material are: 26% to 50% cement, 5% to 30% blast furnace slag, 1.5% to 10% water glass, 0.05% to 1.5% sodium hydroxide, and 35% to 45% water.
4. The grouting reinforcement material for broken rock mass according to any one of claims 1 to 3, characterized in that: The cement comprises the following components by mass percentage: SiO2 22%~23%, Al2O3 4%~5%, CaO 62%~63%, MgO 1.5%~2%, Fe2O3 2%~3%, and SO3 2.5%~3%.
5. The grouting reinforcement material for broken rock mass according to any one of claims 1 to 3, characterized in that: The blast furnace slag includes the following components by mass percentage: SiO2 33%~34%, Al2O3 15%~16%, CaO 37%~38%, MgO 8%~9%, Fe2O3 0.5%~1%, and TiO2 1.5%~2%.
6. The grouting reinforcement material for broken rock mass according to any one of claims 1 to 3, characterized in that: The water glass comprises the following components by mass percentage: SiO2 29%-30%, Na2O 13%-14%, and H2O 56%-57%.
7. The grouting reinforcement material for broken rock mass according to claim 6, characterized in that: The Baume degree of the water glass is 50, and the density of the water glass is 1.48 g / cm 3 , the water glass modulus is 2.
25.
8. The grouting reinforcement material for broken rock mass according to any one of claims 1 to 3, characterized in that: The purity of the sodium hydroxide is at least 96%.
9. The grouting reinforcement material for broken rock mass according to claim 1, characterized in that: The fluidity of the grouting reinforcement material is 334~418mm, the water separation rate is 0.5~4%, the initial setting time is 95~496min, the final setting time is 120~571min, and the compressive strength is 2.24~8.40MPa.
10. A method for preparing the grouting reinforcement material for crushing rock mass according to any one of claims 1 to 9, characterized in that: The preparation method comprises: According to the composition ratio of the raw materials, the masses of various raw materials are weighed, and then the weighed cement and blast furnace slag are mixed and stirred, and water and water glass are mixed and stirred; Pour the stirred solid raw materials and water glass solution into a mixer and stir evenly to obtain a grouting reinforcement material.
Citation Information
Cited By
Quick-setting grouting reinforcement material for coal mine composite roof
CN121913743A