Anti-seepage wall solidifying slurry and preparation method and application thereof
By combining modified chitosan nano-oxide with bentonite, a seepage-proof wall slurry with high dynamic shear force and low filtration loss was prepared, which solved the problems of high cost of bentonite slurry and insufficient performance of polymer slurry, and achieved a more efficient wall stabilization effect.
Patent Information
- Application Number
- CN202411337291.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-25
AI Technical Summary
Existing bentonite mud has the problems of high price and difficulty in waste mud treatment. In addition, polymer mud has a complex composition and low dynamic and static shear strength, making it difficult to effectively replace bentonite and meet the needs of anti-seepage wall construction.
A modified chitosan nano-oxide mixture was prepared by combining modified chitosan nano-oxide with bentonite, soda ash and water, and by calcining nano-zinc oxide, nano-silica and kaolin, which was then used to prepare anti-seepage wall slurry.
It improves the dynamic and static shear force of the drilling mud, enhances its ability to carry and suspend rock cuttings, reduces filtration loss, avoids borehole wall instability and collapse, and provides better borehole cleaning effect.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of advanced new materials, relates to the technical field of new mud building materials, and specifically relates to an anti-seepage wall fixing mud and a preparation method and application thereof. Background Art
[0002] Reservoirs and dams are important parts of water conservancy projects, and the scientific construction of anti-seepage walls is one of the keys to ensuring the quality of water conservancy projects. my country began to use anti-seepage walls for related engineering construction in the 1950s. In 1958, a new method of slot-type concrete anti-seepage construction was created in the gravel foundation of the Miyun Reservoir in Beijing. After the 1970s, anti-seepage wall technology was rapidly popularized in my country, and the anti-seepage wall of the Zhelin Reservoir in Yongxiu, Jiangxi and the anti-seepage wall of the Huangyanghe Reservoir in Wuwei, Gansu were built successively.
[0003] In the construction of anti-seepage walls, the most important function of mud is to fix the wall. At present, the wall-fixing mud widely used in China is bentonite mud. In actual use, in order to meet different requirements, some admixtures are often added, such as dispersants represented by soda ash and caustic soda, thickeners represented by carboxymethyl cellulose, and weighting agents represented by barite powder. Although bentonite mud has the advantages of convenient material acquisition and easy preparation, it also has the disadvantages of high-quality bentonite being expensive and waste slurry being difficult to handle. At the same time, in the prior art, no matter what kind of admixture is added, it has basically no effect on the amount of bentonite added in the bentonite mud. Therefore, how to develop a wall-fixing mud that replaces bentonite or reduces the amount of bentonite added is one of the important research and development directions in this field.
[0004] At present, the main substitute for bentonite mud is polymer mud, such as Neptune polymer mud and AOS foam mud. However, there are few existing polymer muds, and most of them are confidential formulas, which makes the corresponding research and development very difficult. In addition, Neptune polymer mud also has the defects of complex composition and relatively low dynamic shear force and static shear force. Therefore, how to develop a new type of wall-fixing mud that solves the above-mentioned defects is urgently needed in this field. Summary of the invention
[0005] In view of the defects of the prior art, one of the purposes of the present invention is to provide an anti-seepage wall fixing mud which uses a new type of polymer material as a raw material and has high dynamic shear force, static shear force and low filtration loss.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A kind of anti-seepage wall fixing mud, the raw materials of the wall fixing mud include 20-30 parts of bentonite, 10-15 parts of modified chitosan nano oxide mixture, 0.1-0.2 parts of soda ash, and 1000 parts of water by weight;
[0008] Wherein, the preparation method of the modified chitosan nano-oxide mixture comprises the following steps:
[0009] (1) Mix nano zinc oxide, nano silicon dioxide and kaolin in a weight ratio of 5-7:1:1, then calcine at 800-850°C for 60-65 minutes, and grind into powder after cooling;
[0010] (2) dissolving chitosan and lignin nanoparticles in an acetic acid aqueous solution at a weight ratio of 12 to 16:1, such that the weight volume content of chitosan is 1 to 1.5% w / v;
[0011] (3) mixing the product obtained in step (1) and the product obtained in step (2) at a solid-liquid weight ratio of 2.5 to 3:1; after sufficient stirring, adding thiosemicarbazide and stirring, and then adding formaldehyde and continuing to stir until no colloid is generated; then adjusting the pH to alkaline with alkali solution and stirring until no precipitate is generated; washing the precipitate, drying the water, and grinding it into powder.
[0012] Preferably, when preparing the modified chitosan nano-oxide mixture, the weight ratio of nano-zinc oxide, nano-silicon dioxide and kaolin is 6:1:1.
[0013] Preferably, when preparing the modified chitosan nano-oxide mixture, the weight ratio of chitosan to lignin nanoparticles is 14:1.
[0014] Preferably, when preparing the modified chitosan nano-oxide mixture, the concentration of the acetic acid aqueous solution is 1% v / v.
[0015] Preferably, when preparing the modified chitosan nano-oxide mixture, the weight volume content of chitosan is 1.2% w / v; the weight of thiosemicarbazide is half the weight of chitosan; and the volume weight ratio of added formaldehyde to chitosan is 5:1.
[0016] Preferably, when preparing the modified chitosan nano-oxide mixture, the product obtained in step (1) and the product obtained in step (2) are mixed at a solid-liquid weight ratio of 2.8:1.
[0017] Preferably, when preparing the modified chitosan nano-oxide mixture, the drying in step (3) is carried out at 60°C.
[0018] Preferably, the raw materials of the wall-solidifying slurry are composed, by weight, of 25 parts of bentonite, 12 parts of modified chitosan nano-oxide mixture, 0.1 parts of soda ash and 1000 parts of water.
[0019] Another object of the present invention is to provide a method for preparing anti-seepage wall fixing mud, the preparation method comprises preparing the raw materials of the anti-seepage wall fixing mud, first adding the bentonite into water and stirring, then adding the modified chitosan nano oxide mixture and soda ash and continuing to stir.
[0020] Another object of the present invention is to provide an application of the aforementioned anti-seepage wall fixing slurry in anti-seepage wall fixing.
[0021] Beneficial effects of the present invention:
[0022] The anti-seepage wall fixing mud provided by the present invention has higher dynamic shear force and static shear force, and has stronger ability to carry and suspend rock cuttings. It can not only have better hole cleaning effect but also well avoid hole wall instability and collapse, and the filtration loss is relatively small. It is a new type of wall fixing mud compared with traditional bentonite mud and traditional polymer mud, and has good application prospects. DETAILED DESCRIPTION
[0023] In order to better understand the essence of the present invention, the technical content of the present invention is described in detail below with reference to examples, but the content of the present invention is not limited thereto and cannot be understood as limiting the patent scope of the present invention.
[0024] The raw materials involved in the examples of the present invention and the comparative examples are as follows:
[0025] Bentonite: sodium bentonite, Sichuan Yingfan Environmental Technology Co., Ltd.;
[0026] Nano zinc oxide: Chengdu Yishengjin Technology Co., Ltd.;
[0027] Nano-silicon dioxide: Chengdu Nuclear 857 New Materials Co., Ltd.;
[0028] Kaolin: Chengdu Chenzheng Chemical Co., Ltd.;
[0029] Chitosan: content 99%, Chengdu Wanxiang Hongrun Biotechnology Co., Ltd.;
[0030] Lignin nanoparticles: Jinan Shengquan Group Co., Ltd.
[0031] Acetic acid: Own.
[0032] Example 1
[0033] 1. Preparation of modified chitosan nano-oxide mixture raw materials:
[0034] (1) Nano zinc oxide, nano silicon dioxide and kaolin were mixed in a weight ratio of 6:1:1, then calcined at 850°C for 60 minutes, and ground into powder after cooling;
[0035] (2) dissolving chitosan and lignin nanoparticles in an acetic acid aqueous solution (1% v / v) at a weight ratio of 14:1, such that the weight volume content of chitosan is 1.2% w / v;
[0036] (3) Mixing the product of step (1) and the product of step (2) at a solid-liquid weight ratio of 2.8:1; after sufficient stirring, adding thiosemicarbazide accounting for half the weight of chitosan and stirring, then adding formaldehyde and continuing to stir until no colloid is generated, and the volume ratio of the added formaldehyde to the weight of chitosan is 5ml:1g; then adjusting the pH to 10.5 with 30% sodium hydroxide solution and stirring until no precipitate is generated; washing the precipitate with water, drying the water and grinding it into powder.
[0037] 2. Preparation of wall-solidifying slurry:
[0038] Prepare 25 parts of bentonite, 12 parts of modified chitosan nano-oxide mixture, 0.1 parts of soda ash and 1000 parts of water by weight; add one-third of the water into a mixing bucket, add bentonite and stir, and keep adding water during the stirring process; then add the modified chitosan nano-oxide mixture and soda ash and keep stirring.
[0039] Example 2
[0040] 1. Preparation of modified chitosan nano-oxide mixture raw materials:
[0041] (1) Nano zinc oxide, nano silicon dioxide and kaolin were mixed in a weight ratio of 7:1:1, then calcined at 850°C for 60 minutes, and ground into powder after cooling;
[0042] (2) dissolving chitosan and lignin nanoparticles in an acetic acid aqueous solution (1% v / v) at a weight ratio of 12:1, such that the weight volume content of chitosan is 1.5% w / v;
[0043] (3) Mixing the product of step (1) and the product of step (2) at a solid-liquid weight ratio of 3:1; after sufficient stirring, adding thiosemicarbazide accounting for half the weight of chitosan and stirring, then adding formaldehyde and continuing to stir until no colloid is generated, and the volume ratio of the added formaldehyde to the weight of chitosan is 5ml:1g; then adjusting the pH to 10.5 with 30% sodium hydroxide solution and stirring until no precipitate is generated; washing the precipitate with water, drying the water and grinding it into powder.
[0044] 2. Preparation of wall-solidifying slurry:
[0045] Prepare 20 parts of bentonite, 15 parts of modified chitosan nano-oxide mixture, 0.1 parts of soda ash and 1000 parts of water by weight; add one-third of the water into a mixing bucket, add bentonite and stir, and keep adding water during the stirring process; then add the modified chitosan nano-oxide mixture and soda ash and keep stirring.
[0046] Example 3
[0047] 1. Preparation of modified chitosan nano-oxide mixture raw materials:
[0048] (1) Nano zinc oxide, nano silicon dioxide and kaolin were mixed in a weight ratio of 5:1:1, then calcined at 800°C for 65 minutes, and ground into powder after cooling;
[0049] (2) dissolving chitosan and lignin nanoparticles in an acetic acid aqueous solution (1% v / v) at a weight ratio of 16:1, such that the weight volume content of chitosan is 1% w / v;
[0050] (3) Mixing the product of step (1) and the product of step (2) at a solid-liquid weight ratio of 2.5:1; after sufficient stirring, adding thiosemicarbazide accounting for half the weight of chitosan and stirring, then adding formaldehyde and continuing to stir until no colloid is generated, and the volume ratio of the added formaldehyde to the weight of chitosan is 5ml:1g; then adjusting the pH to 10.5 with 30% sodium hydroxide solution and stirring until no precipitate is generated; washing the precipitate with water, drying the water and grinding it into powder.
[0051] 2. Preparation of wall-solidifying slurry:
[0052] Prepare 30 parts of bentonite, 10 parts of modified chitosan nano-oxide mixture, 0.2 parts of soda ash and 1000 parts of water by weight; add one-third of the water into a mixing bucket, add bentonite and stir, and continuously add water during the stirring process; then add the modified chitosan nano-oxide mixture and soda ash and continue stirring.
[0053] Comparative Example 1
[0054] When preparing the modified chitosan nano-oxide mixture, nano zinc oxide was not added, and the rest was consistent with Example 1.
[0055] The specific scheme of this comparative example is as follows:
[0056] 1. Preparation of modified chitosan nano-oxide mixture raw materials:
[0057] (1) Nano zinc oxide and kaolin were mixed in a weight ratio of 6:1, then calcined at 850°C for 60 minutes, and ground into powder after cooling;
[0058] (2) dissolving chitosan and lignin nanoparticles in an acetic acid aqueous solution (1% v / v) at a weight ratio of 14:1, such that the weight volume content of chitosan is 1.2% w / v;
[0059] (3) Mixing the product of step (1) and the product of step (2) at a solid-liquid weight ratio of 2.8:1; after sufficient stirring, adding thiosemicarbazide accounting for half the weight of chitosan and stirring, then adding formaldehyde and continuing to stir until no colloid is generated, and the volume ratio of the added formaldehyde to the weight of chitosan is 5ml:1g; then adjusting the pH to 10.5 with 30% sodium hydroxide solution and stirring until no precipitate is generated; washing the precipitate with water, drying the water and grinding it into powder.
[0060] 2. Preparation of wall-solidifying slurry:
[0061] Prepare 25 parts of bentonite, 12 parts of modified chitosan nano-oxide mixture, 0.1 parts of soda ash and 1000 parts of water by weight; add one-third of the water into a mixing bucket, add bentonite and stir, and keep adding water during the stirring process; then add the modified chitosan nano-oxide mixture and soda ash and keep stirring.
[0062] Comparative Example 2
[0063] The difference between this comparative example and Example 1 is that no kaolin is added and no calcination treatment is performed.
[0064] The specific scheme of this comparative example is as follows:
[0065] 1. Preparation of modified chitosan nano-oxide mixture raw materials:
[0066] (1) Mix nano zinc oxide and nano silicon dioxide in a weight ratio of 6:1;
[0067] (2) dissolving chitosan and lignin nanoparticles in an acetic acid aqueous solution (1% v / v) at a weight ratio of 14:1, such that the weight volume content of chitosan is 1.2% w / v;
[0068] (3) Mixing the product of step (1) and the product of step (2) at a solid-liquid weight ratio of 2.8:1; after sufficient stirring, adding thiosemicarbazide accounting for half the weight of chitosan and stirring, then adding formaldehyde and continuing to stir until no colloid is generated, and the volume ratio of the added formaldehyde to the weight of chitosan is 5ml:1g; then adjusting the pH to 10.5 with 30% sodium hydroxide solution and stirring until no precipitate is generated; washing the precipitate with water, drying the water and grinding it into powder.
[0069] 2. Preparation of wall-solidifying slurry:
[0070] Prepare 25 parts of bentonite, 12 parts of modified chitosan nano-oxide mixture, 0.1 parts of soda ash and 1000 parts of water by weight; add one-third of the water into a mixing bucket, add bentonite and stir, and keep adding water during the stirring process; then add the modified chitosan nano-oxide mixture and soda ash and keep stirring.
[0071] Comparative Example 3
[0072] When preparing the modified chitosan nano-oxide mixture, the process was the same as in Example 1 except that no lignin nanoparticles were added.
[0073] The specific scheme of this comparative example is as follows:
[0074] 1. Preparation of modified chitosan nano-oxide mixture raw materials:
[0075] (1) Nano zinc oxide, nano silicon dioxide and kaolin were mixed in a weight ratio of 6:1:1, then calcined at 850°C for 60 minutes, and ground into powder after cooling;
[0076] (2) dissolving chitosan in an acetic acid aqueous solution (1% v / v) so that the weight volume content of chitosan is 1.2% w / v;
[0077] (3) Mixing the product of step (1) and the product of step (2) at a solid-liquid weight ratio of 2.8:1; after sufficient stirring, adding thiosemicarbazide accounting for half the weight of chitosan and stirring, then adding formaldehyde and continuing to stir until no colloid is generated, and the volume ratio of the added formaldehyde to the weight of chitosan is 5ml:1g; then adjusting the pH to 10.5 with 30% sodium hydroxide solution and stirring until no precipitate is generated; washing the precipitate with water, drying the water and grinding it into powder.
[0078] 2. Preparation of wall-solidifying slurry:
[0079] Prepare 25 parts of bentonite, 12 parts of modified chitosan nano-oxide mixture, 0.1 parts of soda ash and 1000 parts of water by weight; add one-third of the water into a mixing bucket, add bentonite and stir, and keep adding water during the stirring process; then add the modified chitosan nano-oxide mixture and soda ash and keep stirring.
[0080] Comparative Example 4
[0081] When preparing the modified chitosan nano-oxide mixture, no treatment with thiosemicarbazide and formaldehyde was performed, and only physical mixing was performed. The rest was consistent with Example 1.
[0082] The specific scheme of this comparative example is as follows:
[0083] 1. Preparation of chitosan nano-oxide mixture raw materials:
[0084] (1) Nano zinc oxide, nano silicon dioxide and kaolin were mixed in a weight ratio of 6:1:1, then calcined at 850°C for 60 minutes, and ground into powder after cooling;
[0085] (2) dissolving chitosan and lignin nanoparticles in an acetic acid aqueous solution (1% v / v) at a weight ratio of 14:1, such that the weight volume content of chitosan is 1.2% w / v;
[0086] (3) The product obtained in step (1) and the product obtained in step (2) were mixed at a solid-liquid weight ratio of 2.8:1; after sufficient stirring, most of the water was naturally evaporated at 60° C., and then the remaining water was removed by a rotary evaporator, and then ground into powder.
[0087] 2. Preparation of wall-solidifying slurry:
[0088] Prepare 25 parts of bentonite, 12 parts of chitosan nano-oxide mixture, 0.1 parts of soda ash and 1000 parts of water by weight; add one-third of the water into a mixing bucket, add bentonite and stir, and keep adding water during the stirring process; then add the modified chitosan nano-oxide mixture and soda ash and keep stirring.
[0089] Experimental Example 1
[0090] The Marsh funnel viscosity, plastic viscosity, apparent viscosity, dynamic shear force, static shear force, filtration loss and pH value of the muds obtained in Examples 1-3 and Comparative Examples 1-4 were investigated.
[0091] Through the rotational viscometer test, φ600, φ300, and φ3 are the readings on the instrument dial at 600, 300, and 3 r / min respectively.
[0092] Plastic viscosity η P =φ600-φ300(mPa·s);
[0093] Apparent viscosity η A =0.5×φ600(mPa·s);
[0094] Dynamic shear force η d =0.511×(φ300-η P )(Pa);
[0095] Static shear force (10min) τ 10 =0.511×φ3(Pa).
[0096] The air pressure mud water loss meter is used at a working pressure of 0.7 MPa. Filter paper is used as the filtration medium. The filtration loss within 30 minutes is measured as the filtration loss in mL / min.
[0097] Table 1
[0098]
[0099] As shown in Table 1, Examples 1-3 of the present invention have higher dynamic shear force and static shear force, and have stronger ability to carry and suspend rock cuttings. They can not only have better hole cleaning effect but also well avoid hole wall instability and collapse, and the filtration loss is relatively small.
[0100] Generally speaking, the wall-fixing mud of the anti-seepage wall usually adopts bentonite, clay and chemical mud. Among them, bentonite is used more frequently. For example, Yin Hong selected bentonite, sodium carbonate and carboxymethyl cellulose to prepare the wall-fixing mud in the paper "Preparation and Construction of Anti-seepage Wall Fixing Mud"; Zhang Boyi et al. designed different mud formulas using bentonite, soda ash, thickener and dispersant in the paper "Mud Improvement and Application in the Construction of Fine Sand Layer Anti-seepage Wall" and investigated the application effect; Zhang Qihe et al. also discussed the effect of using bentonite, sodium carbonate, carboxymethyl cellulose and barite powder to prepare the wall-fixing mud in the paper "Overview of the Reinforcement Mud System of the Anti-seepage Wall of the No. 8 Auxiliary Dam of Lushui Reservoir"; similarly, Zhang Xuanzhuang et al. also used bentonite to prepare the wall-fixing mud in the paper "Productive Test Research on the Anti-seepage Wall of a Dam Foundation of a Reservoir".
[0101] When using bentonite, people also investigated other pulping raw materials. For example, Wan Wencai summarized the available dispersants, viscosity enhancers and weighting agents in his paper "Application of Mud Wall Fixing Technology in Reservoir Anti-seepage Wall Construction". In addition to the commonly used soda ash, caustic soda and carboxymethyl cellulose, people also investigated other pulping raw materials. For example, Dai Guozhong et al. used polymers as raw materials in their paper "Mulch Material Preparation and Wall Forming Process of Wall Mud Anti-seepage Wall". Specifically, hydrolyzed polyacrylamide and hydrolyzed polyacrylonitrile were used in combination with bentonite and soda ash to prepare wall fixing mud. However, the dynamic shear force of the mud obtained was very low, only 1.2~3Pa.
[0102] In terms of the use of polymers, Zhou Changmao and others introduced the application effect of Neptune polymer mud in the paper "Application of polymer mud in the anti-seepage wall project of Houziyan Hydropower Station". Its configuration is simple, and only Neptune polymer and alkali need to be added to water to make mud. However, its composition has not been fully disclosed, and it is difficult for people to develop corresponding alternative products. From the current information, the mud is mainly composed of polymers such as emulsified asphalt, styrene-acrylic emulsion and polyurethane.
[0103] Through constant exploration, the inventors found that the performance of the wall-fixing mud obtained by the present invention is good, and the addition amount of bentonite can be effectively reduced. Importantly, the present invention obtains a wall-fixing mud that can be used in conjunction with bentonite by chemically modifying chitosan and blending and modifying it with other substances. As shown in the aforementioned related comparative examples, the selection of kaolin, nano oxide and lignin nano particles has a great influence on the performance of the wall-fixing mud. The possible reason is that the addition of fine particles makes the mud skin dense, increases shear force and reduces water loss, but the specific selection of fine particles needs to be considered to better play a role with modified chitosan. At the same time, the nano oxide is tightly bonded to kaolin by roasting, the surface properties of the nano particles are changed, and the interaction with the modified chitosan is improved. In addition, the addition of lignin nano particles may change the surface properties of chitosan when it is modified into a gel and precipitated, further promoting the combination with the nano particles.
[0104] In summary, the wall-fixing mud provided by the present invention significantly reduces the amount of bentonite added, while the prior art generally requires 50 to 60 g of bentonite for every 1000 g of water; and by modifying the inorganic nanoparticles and combining them with modified chitosan, the dynamic shear force and static shear force performance of the wall-fixing mud are effectively improved, and the filtration loss is lower. The wall-fixing mud is different from the traditional bentonite or clay mud and the traditional polymer mud.
Claims
1. A kind of anti-seepage wall fixing mud, characterized in that: The raw materials of the wall-fixing mud include, by weight, 20 to 30 parts of bentonite, 10 to 15 parts of modified chitosan nano-oxide mixture, 0.1 to 0.2 parts of soda ash, and 1000 parts of water; Wherein, the preparation method of the modified chitosan nano-oxide mixture comprises the following steps: (1) Mix nano zinc oxide, nano silicon dioxide and kaolin in a weight ratio of 5-7:1:1, then calcine at 800-850°C for 60-65 minutes, and grind into powder after cooling; (2) dissolving chitosan and lignin nanoparticles in an acetic acid aqueous solution at a weight ratio of 12 to 16:1, such that the weight volume content of chitosan is 1 to 1.5% w / v; (3) Mixing the product of step (1) and the product of step (2) at a solid-liquid weight ratio of 2.5 to 3:1; after sufficient stirring, adding thiosemicarbazide accounting for half the weight of chitosan and stirring, then adding formaldehyde and continuing to stir until no colloid is generated, and the volume ratio of the added formaldehyde to the weight of chitosan is 5 ml:1 g; then adjusting the pH to alkaline with 30% sodium hydroxide solution and stirring until no precipitate is generated; washing the precipitate, drying the water and grinding it into powder.
2. The anti-seepage wall fixing slurry according to claim 1, characterized in that: When preparing the modified chitosan nano-oxide mixture, the weight ratio of nano zinc oxide, nano silicon dioxide and kaolin is 6:1:
1.
3. The anti-seepage wall fixing slurry according to claim 2, characterized in that: When preparing the modified chitosan nano-oxide mixture, the weight ratio of chitosan and lignin nanoparticles is 14:
1.
4. The anti-seepage wall fixing slurry according to claim 3, characterized in that: When preparing the modified chitosan nano-oxide mixture, the concentration of the acetic acid aqueous solution is 1% v / v.
5. The anti-seepage wall fixing slurry according to claim 4, characterized in that: When preparing the modified chitosan nano-oxide mixture, the weight volume content of chitosan is 1.2% w / v; the weight of aminothiourea is half of the weight of chitosan; and the volume weight ratio of added formaldehyde to chitosan is 5:
1.
6. The anti-seepage wall fixing slurry according to claim 5, characterized in that: When preparing the modified chitosan nano-oxide mixture, the product obtained in step (1) and the product obtained in step (2) are mixed at a solid-liquid weight ratio of 2.8:
1.
7. The anti-seepage wall fixing slurry according to claim 1 or 6, characterized in that: When preparing the modified chitosan nano-oxide mixture, the drying in step (3) is carried out at 60°C.
8. The anti-seepage wall fixing slurry according to claim 7, characterized in that: The raw materials of the wall-fixing mud are composed of 25 parts of bentonite, 12 parts of modified chitosan nano-oxide mixture, 0.1 parts of soda ash and 1000 parts of water in parts by weight.
9. A method for preparing anti-seepage wall solidifying slurry, characterized in that: The preparation method comprises preparing the raw materials of the anti-seepage wall fixing mud according to any one of claims 1 to 8, firstly adding the bentonite into water and stirring, and then adding the modified chitosan nano-oxide mixture and soda ash and continuing to stir.
10. Use of the anti-seepage wall consolidation slurry according to any one of claims 1 to 8 in consolidating anti-seepage walls.