Carbon sequestration type permeable ecological concrete as well as preparation method and application thereof
By using sulphoaluminate cement, modified porous coarse aggregate and polycarboxylate superplasticizer in the preparation of carbon-fixing permeable ecological concrete, combined with modified mixing water treatment and carbonization curing, the mechanical properties of traditional ecological concrete are solved. and the problem of insufficient alkalinity, we have achieved high strength, water permeability and environmentally friendly carbon-fixing permeable ecological concrete, which is suitable for plant growth and avoids pollution.
Patent Information
- Application Number
- CN202410940303.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-29
AI Technical Summary
Traditional ecological concrete has deficiencies in mechanical properties and alkalinity, which limits its promotion and application in engineering, and existing alkali reduction methods pose environmental pollution risks.
The preparation method of carbon-fixing permeable ecological concrete is adopted, including the use of sulphoaluminate cement, modified porous coarse aggregate, admixtures and polycarboxylate superplasticizer, and through modified mixing water treatment and carbonization curing, it is prepared Carbon-fixing permeable ecological concrete with high strength and suitable alkalinity.
It achieves high strength and high water permeability carbon-fixing permeable ecological concrete, which overcomes the high alkalinity defect of traditional concrete and is suitable for the growth of most plants while avoiding environmental pollution.
Smart Images

Figure BDA0004943864730000061 
Figure BDA0004943864730000062 
Figure BDA0004943864730000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete, and in particular to a carbon-fixing type water-permeable ecological concrete and a preparation method and application thereof. Background Art
[0002] Ecological concrete is a building material that is made of specially graded coarse aggregate, cement, admixtures and water in a certain proportion. It can drain water quickly and has a certain strength. It is also called ecological porous concrete and permeable concrete. It is widely used in construction projects, road projects, slope protection projects and sponge city construction. The porosity of its structure and its good water permeability and air permeability allow vegetation to grow naturally on or in it. Therefore, it is widely used in river bank protection, parking lots, green roofs and other fields. The main defect of traditional ecological concrete is that the internal environment of concrete is highly alkaline, and the materials are mostly in point contact, which is easy to produce stress concentration when subjected to force. Therefore, its mechanical properties are generally lower than those of ordinary concrete, which limits its promotion and application in engineering. For example, the Chinese invention patent application with document number CN115700231A discloses a porous ecological concrete and its preparation process. The technical scheme adopted is mainly as follows: silica fume and ferrous sulfate are used in combination. The silica fume consumes soluble alkaline substances such as calcium hydroxide produced by cement hydration and fixes insoluble alkali. Ferrous sulfate improves the compressive strength and the alkali-reducing effect of silica fume. It is also combined with a reinforcing agent prepared from fluorosulfuric acid, potassium hydrogen sulfate, sodium hydrogen sulfate and potassium aluminum sulfate. The reinforcing agent hydrolyzes to produce an alkali-inhibiting product, thereby effectively reducing the alkalinity of the cement-based cementitious material, so that the alkalinity of the prepared porous concrete is roughly maintained at around pH 9. The Chinese invention patent with the document number CN109400208B discloses a process for reducing the alkalinity of ecological concrete by silane impregnation, so that the pH of the prepared ecological concrete can be maintained at about 8.5, which can meet the needs of most plant growth. However, organic silane is highly volatile and easily volatilizes into organic silane vapor, which can directly harm the human respiratory and digestive systems. In addition, when organic silane enters water bodies and soil, it will directly cause environmental pollution. Therefore, the development of efficient and safe ecological concrete alkalinity reduction methods is an urgent problem to be solved. Summary of the invention
[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a carbon-fixing permeable ecological concrete and a preparation method and application thereof. The carbon-fixing permeable ecological concrete has high mechanical strength and appropriate alkalinity, which is conducive to plant cultivation.
[0004] In order to achieve the above technical effects, the present invention adopts the following technical solutions:
[0005] In a first aspect, the present invention provides a carbon-fixing permeable ecological concrete, which comprises the following components by mass: 110 to 160 parts of sulphoaluminate cement, 280 to 320 parts of modified porous coarse aggregate, 55 to 75 parts of admixture, 1 to 3 parts of additives and 40 to 70 parts of water.
[0006] Preferably, the modified porous coarse aggregate is a mixture of any one or more of modified porous ceramsite, modified expanded perlite or modified coral aggregate.
[0007] Preferably, the auxiliary agent is a water reducer, and the water reducer is preferably a polycarboxylate water reducer PCA.
[0008] Preferably, the admixture is composed of the following raw materials in parts by mass: 10 to 15 parts of silica fume, 5 to 10 parts of fly ash, 12 to 25 parts of limestone and 5 to 8 parts of lithium carbonate.
[0009] In a second aspect, the present invention further provides a method for preparing the carbon-fixing permeable ecological concrete provided in the first aspect, comprising the following steps:
[0010] S1: preparing cement slurry, wherein the cement slurry comprises sulphoaluminate cement, admixtures and 1 / 2 to 2 / 3 of water;
[0011] S2: preparing modified porous coarse aggregate, wherein the porous coarse aggregate is a mixture of any one or more of sintered porous ceramsite, expanded perlite, and porous coral aggregate;
[0012] S3: mixing the modified porous coarse aggregate and cement slurry to prepare a primary concrete mix;
[0013] S4: adding a water reducing agent and the remaining water in the formula to the primary concrete mixture, mixing and stirring uniformly to obtain a concrete slurry, pouring and curing the concrete slurry to obtain a concrete embryo, and carbonizing and curing the embryo to obtain a carbon-fixing permeable ecological concrete.
[0014] Furthermore, the preparation method of the modified porous coarse aggregate is as follows:
[0015] S2-1: preparing modified mixing water, wherein the modified mixing water includes a surfactant, ferrous sulfate, urea, calcium hydroxide, sodium hexametaphosphate and aluminum chloride;
[0016] S2-2: The porous coarse aggregate is immersed in modified mixed water at a material-liquid ratio of 1:15 to 18, and taken out after immersion for 10 to 30 minutes. After draining the water, the modified porous coarse aggregate is dried at 50° C. or air-dried to obtain the modified porous coarse aggregate.
[0017] Preferably, the surfactant is a mixture of sodium lauryl sulfate and sodium cetyl phosphate.
[0018] Furthermore, the composition of the modified mixing water is as follows in parts by mass:
[0019] 0.3-0.5 parts of surfactant, 5-8 parts of ferrous sulfate, 1-2 parts of urea, 21-32 parts of calcium hydroxide, 1-2 parts of sodium hexametaphosphate, 2-5 parts of aluminum chloride and 300-350 parts of water.
[0020] Preferably, the porous coarse aggregate is a mixture of modified coral aggregate and modified porous ceramsite.
[0021] Preferably, the carbonization curing conditions are: controlling the curing temperature to 20-25° C. and the relative humidity to 70%-90%, pre-curing for 10-30 hours, and then introducing carbon dioxide gas with a carbon dioxide volume concentration of ≥80%, and continuing the curing for 10-20 hours.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention provides a carbon-fixing type permeable ecological concrete, which is composed of 110 to 160 parts of sulphoaluminate cement, 280 to 320 parts of modified porous coarse aggregate, 55 to 75 parts of admixture, 1 to 3 parts of water reducer and 40 to 70 parts of water. In the preparation process of the carbon-fixing type permeable ecological concrete, the inventor adopts porous coarse aggregate and modified mixing water for mixing and modifying to obtain modified porous coarse aggregate, and then uses the modified porous coarse aggregate to prepare the carbon-fixing type permeable ecological concrete. At the same time, the composition and proportion of the admixture are adjusted. The preparation of high-strength and high-permeability carbon-fixing type permeable ecological concrete is achieved through the combination of the modified porous coarse aggregate and the admixture, and the carbon-fixing type permeable ecological concrete can overcome the defect of high alkalinity in traditional carbon-fixing type permeable ecological concrete, and is more conducive to the growth of most plants. DETAILED DESCRIPTION
[0024] The following embodiments are only used to more clearly illustrate the technical solutions of the present invention and are therefore only used as examples and are not intended to limit the scope of protection of the present invention.
[0025] For those skilled in the art, any equivalent modifications and substitutions to the embodiments described below are also within the scope of the present invention. Therefore, the equalization and modification made without departing from the spirit and scope of the present invention should be included in the scope of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for all reagents or instruments, they are all conventional products that can be purchased commercially.
[0026] In order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other embodiments, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art. Unless otherwise specified, the units used in this specification are all international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0028] Example 1
[0029] The present embodiment provides a carbon-fixing permeable ecological concrete, which comprises the following components by weight: 130 parts of sulphoaluminate cement, 300 parts of modified porous coarse aggregate, 60 parts of admixture, 1.5 parts of polycarboxylate water-reducing agent PCA and 55 parts of water;
[0030] The admixtures are composed of 13 parts of silica fume, 5 parts of fly ash, 12 parts of limestone and 6 parts of lithium carbonate in terms of mass.
[0031] Specifically, the preparation method of the carbon-fixing permeable ecological concrete is as follows:
[0032] S1: preparing cement slurry, wherein the cement slurry comprises sulphoaluminate cement, admixtures and 1 / 2 weight of water;
[0033] S2: Prepare modified porous coarse aggregate, the specific method is:
[0034] S2-1: Prepare modified mixing water, the composition of the modified mixing water is as follows:
[0035] 0.4 parts of surfactant (sodium lauryl sulfate), 7 parts of ferrous sulfate, 1.5 parts of urea, 27 parts of calcium hydroxide, 1.7 parts of sodium hexametaphosphate, 4 parts of aluminum chloride and 330 parts of water;
[0036] The preparation method of the modified mixing water is as follows: weigh the raw materials according to the above formula and mix them with water to obtain;
[0037] S2-2: Immerse the porous coarse aggregate (porous ceramsite and porous coral aggregate in a mass ratio of 1:2) in modified mixing water at a material-liquid ratio of 1:15, take out after soaking for 15 minutes, drain the water and dry at a constant temperature of 45°C to obtain the modified porous coarse aggregate.
[0038] S3: mixing the modified porous coarse aggregate and cement slurry to prepare a primary concrete mix;
[0039] S4: adding a water reducing agent and the remaining water in the formula to the concrete primary mixture, mixing and stirring uniformly to obtain a concrete slurry, pouring and curing the concrete slurry to obtain a concrete embryo, and carbonizing and curing the embryo to obtain a carbon-fixing permeable ecological concrete. Specifically, the carbonization curing conditions are:
[0040] The prepared embryo body was placed in a curing device, and the curing temperature was controlled at 20-25°C and the relative humidity was 80%. After pre-curing for 24 hours, carbon dioxide gas with a volume concentration of ≥80% was introduced into the embryo body and cured for 16 hours to obtain carbon-fixing permeable ecological concrete, which was recorded as sample I.
[0041] Example 2
[0042] The present embodiment provides a carbon-fixing permeable ecological concrete, which includes the following components by mass: 110 parts of sulphoaluminate cement, 280 parts of modified porous coarse aggregate, 55 parts of admixture, 1.2 parts of polycarboxylate water-reducing agent PCA and 40 parts of water. The remaining components and preparation methods are the same as in Example 1, and sample II is obtained.
[0043] Example 3
[0044] The present embodiment provides a carbon-fixing permeable ecological concrete, which includes the following components by mass: 160 parts of sulphoaluminate cement, 320 parts of modified porous coarse aggregate, 75 parts of admixture, 1.4 parts of polycarboxylate water-reducing agent PCA and 70 parts of water. The remaining components and preparation methods are the same as in Example 1, and sample III is obtained.
[0045] Test Example 1
[0046] In this test example, the strength test (including compressive strength and flexural strength), water permeability coefficient and alkalinity test were carried out on the 28th day after the samples were prepared. The test results are shown in Table 1:
[0047] Table 1 Test results of strength and water permeability of samples I to III
[0048]
[0049] Test Example 2
[0050] This embodiment provides a composition and preparation method of a carbon-fixing permeable ecological concrete, which comprises the following components by mass (the composition of the components is the same as that of Example 1): 130 parts of sulphoaluminate cement, 300 parts of modified porous coarse aggregate, 60 parts of admixture, 1.5 parts of polycarboxylate water-reducing agent PCA and 55 parts of water;
[0051] On the basis of Example 1, this example further tests the composition of the admixture, and sets up 8 experimental groups in total. The composition of the admixture of each experimental group is shown in Table 3. The preparation method of each group refers to Example 1. The prepared samples are recorded as Group 1 to Group 8, respectively. The strength test, water permeability coefficient and alkalinity of each group of samples are tested. The experimental results are shown in Table 3:
[0052] Table 3 Effect of admixture composition on the performance of carbon-fixing permeable ecological concrete
[0053]
[0054] It can be seen from the above experiments that the composition of the admixture has a great influence on the compressive strength and flexural strength of the carbon-fixing permeable ecological concrete. Especially when lithium carbonate is not added to the admixture, not only the strength of the sample is poor, but also the alkalinity is high, which is not suitable for plant growth; in the experimental group where fly ash, limestone and lithium carbonate are added at the same time (Group 3 without adding silica fume), although the ecological concrete sample shows good strength, the water permeability coefficient of the sample is poor, the porosity is poor, and the alkalinity is also high.
[0055] Test Example 3
[0056] The present embodiment provides a composition and preparation method of a carbon-fixing permeable ecological concrete. The carbon-fixing permeable ecological concrete comprises the following components by mass (the composition of the components is the same as that of Example 1): 130 parts of sulphoaluminate cement, 300 parts of modified porous coarse aggregate, 60 parts of admixture (the admixture composition in Example 1: 13 parts of silica fume, 5 parts of fly ash, 12 parts of limestone and 6 parts of lithium carbonate), 1.5 parts of polycarboxylate water reducer PCA and 55 parts of water;
[0057] On the basis of Example 1, this example further tests the effect of the composition of modified mixing water on the performance of carbon-fixing permeable ecological concrete. Specifically, this example sets up 7 experimental groups, each of which is recorded as Group 1 to Group 7. The composition of each group of modified mixing water and the test results of the prepared sample performance are shown in Table 4:
[0058] Table 4 Composition of modified mixing water of Group 1 to Group 7
[0059]
[0060] The porous coarse aggregate (the same composition as in Example 1) was modified using the mixing water of the above-mentioned Groups 1 to 7, and the carbon-fixing permeable ecological concrete was prepared using the prepared modified porous coarse aggregate (the preparation method refers to Example 1), and the performance of the prepared concrete samples was tested. The test results are shown in Table 5:
[0061] Table 5 Effect of modified mixing water composition on concrete properties
[0062]
[0063] The above experimental results show that the modified effect of the modified mixing water composition on the porous coarse aggregate can have a significant impact on the performance of the concrete sample. The influencing factors mainly include: the composition of the surfactant, the addition amount of sodium hexametaphosphate and aluminum chloride, and the experimental results show that only when sodium hexametaphosphate and aluminum chloride are added at the same time and the ratio of the two is appropriate, the strength and alkalinity of the concrete can be taken into account. As for the composition of the surfactant, when sodium dodecyl sulfate and sodium hexadecyl phosphate are added as surfactants in a mass ratio of 1:1, the strength of the prepared concrete is greatly affected, indicating that the type of surfactant has a certain influence on the modification effect of porous coarse aggregate. Therefore, in the actual application process, how to choose a suitable surfactant is worth further exploration.
[0064] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it should be understood by those skilled in the art that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention. The techniques, shapes, and structural parts not described in detail in the present invention are all known technologies.
Claims
1. A carbon-fixing permeable ecological concrete, It is characterized in that The invention comprises the following components by weight: 110-160 parts of sulphoaluminate cement, 280-320 parts of modified porous coarse aggregate, 55-75 parts of admixture, 1-3 parts of auxiliary agent and 40-70 parts of water.
2. A carbon-fixing permeable ecological concrete as claimed in claim 1, Features: The modified porous coarse aggregate is a mixture of any one or more of modified porous ceramsite, modified expanded perlite or modified coral aggregate.
3. The carbon-fixing permeable ecological concrete according to claim 1, Features: The auxiliary agent is a water reducer, and the water reducer is preferably a polycarboxylate water reducer PCA.
4. The carbon-fixing permeable ecological concrete according to claim 1, Features: The admixture is composed of the following raw materials in parts by mass: 10 to 15 parts of silica fume, 5 to 10 parts of fly ash, 12 to 25 parts of limestone and 5 to 8 parts of lithium carbonate.
5. A method for preparing a carbon-fixing permeable ecological concrete according to claim 1, It is characterized in that The following steps are involved: S1: preparing cement slurry, wherein the cement slurry comprises sulphoaluminate cement, admixtures and 1 / 2 to 2 / 3 of water; S2: preparing modified porous coarse aggregate, wherein the porous coarse aggregate is a mixture of any one or more of sintered porous ceramsite, expanded perlite, and porous coral aggregate; S3: mixing the modified porous coarse aggregate and cement slurry to prepare a primary concrete mix; S4: adding a water reducing agent and the remaining water in the formula to the primary concrete mixture, mixing and stirring uniformly to obtain a concrete slurry, pouring and curing the concrete slurry to obtain a concrete embryo, and carbonizing and curing the embryo to obtain a carbon-fixing permeable ecological concrete.
6. A method for preparing a carbon-fixing permeable ecological concrete as claimed in claim 5, It is characterized in that The preparation method of the modified porous coarse aggregate is as follows: S2-1: preparing modified mixing water, wherein the modified mixing water includes a surfactant, ferrous sulfate, urea, calcium hydroxide, sodium hexametaphosphate and aluminum chloride; S2-2: The porous coarse aggregate is immersed in modified mixed water at a material-liquid ratio of 1:15 to 18, and taken out after immersion for 10 to 30 minutes. After draining the water, the modified porous coarse aggregate is dried at 50° C. or air-dried to obtain the modified porous coarse aggregate.
7. A method for preparing a carbon-fixing permeable ecological concrete according to claim 6, It is characterized in that The surfactant is a mixture of sodium lauryl sulfate and sodium cetyl phosphate.
8. A method for preparing a carbon-fixing permeable ecological concrete as claimed in claim 7, It is characterized in that The composition of the modified mixing water is as follows in parts by mass: 0.3-0.5 parts of surfactant, 5-8 parts of ferrous sulfate, 1-2 parts of urea, 21-32 parts of calcium hydroxide, 1-2 parts of sodium hexametaphosphate, 2-5 parts of aluminum chloride and 300-350 parts of water.
9. A method for preparing a carbon-fixing permeable ecological concrete according to claim 7, It is characterized in that The carbonization curing conditions are as follows: controlling the curing temperature at 20-25° C. and the relative humidity at 70%-90%, pre-curing for 10-30 hours, and then introducing carbon dioxide gas with a carbon dioxide volume concentration of ≥80% and continuing the curing for 10-20 hours.
10. Application of the carbon-fixing permeable ecological concrete as claimed in claim 1 in construction projects.