A kind of aerogel thermal insulation layer and preparation method thereof
By introducing hydrated aluminum silicate nanofibers and alumina and zirconia composite sols into the aerogel insulation layer material, the problem of insufficient heat resistance temperature and mechanical properties in thermal runaway protection of lithium-ion batteries is solved, and high temperature resistance and The thermal insulation layer with excellent mechanical properties effectively prevents the battery from getting out of control and flame spread.
Patent Information
- Application Number
- CN202411350554.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The existing aerogel insulation layer materials have problems such as insufficient heat resistance temperature and insufficient high temperature mechanical properties in the thermal runaway protection of lithium-ion batteries, which are difficult to effectively prevent catastrophic thermal runaway and flame spread of the battery.
The composite sol preparation method of hydrated aluminum silicate nanofibers, alumina, zirconia and silica is prepared by five-step process: dispersion of hydrated aluminum silicate nanofibers, sol preparation, aging and replacement, drying and heat treatment, and high temperature resistance is prepared. Aerogel thermal insulation layer with excellent mechanical properties.
It significantly improves the temperature resistance limit of the aerogel thermal insulation layer to above 1000℃, and maintains good mechanical properties at high temperatures. It is suitable for thermal runaway protection of lithium-ion batteries, delaying or preventing heat transfer and flame spread.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to an aerogel heat insulation layer and a preparation method thereof, belonging to the technical field of battery protection. Background Art
[0002] Aerogel is a porous material with gas as the dispersion medium. The thermal conductivity of the aerogel insulation layer made of it is about 0.020W / (m·K), and it has the advantages of super hydrophobicity, V0 flame retardant, wide operating temperature range, long life, non-toxic and environmentally friendly. Compared with traditional thermal insulation materials, under the same thermal insulation effect, the thickness of aerogel materials is only 1 / 2~1 / 5 of that of traditional thermal insulation materials. Especially in the thermal insulation effect and flame retardant performance under ultra-high temperature environment, it has advantages that other traditional thermal insulation materials cannot match. This advantage has brought great benefits to solving the problem of thermal runaway protection of lithium-ion batteries. Especially with the rapid development of new energy vehicles, the solution to the problem of thermal runaway protection of lithium-ion batteries is more urgent. When lithium-ion batteries are hit, punctured or short-circuited inside the battery, the heat will increase sharply, causing thermal runaway, and eventually causing fire or explosion. And when a single battery cell has thermal runaway, the heat will be quickly transferred to the adjacent battery cell, causing a series of chain reactions, leading to thermal runaway of the entire module or even the entire battery pack. Using aerogel insulation material to delay or prevent heat diffusion and flame spread of battery packs is a very effective means. Compared with traditional thermal insulation materials such as glass fiber wool, aluminum silicate wool, composite insulation boards, etc., aerogel has lower thermal conductivity, can be reduced in thickness, and has more significant advantages in fire and water resistance. In addition, aerogel has a long service life and its fire resistance and thermal insulation performance hardly decays during its life cycle.
[0003] Although aerogel insulation materials are very suitable for thermal runaway protection of lithium-ion batteries, the silica aerogel currently used on the market, although it has a relatively good protective effect, is still difficult to completely avoid the occurrence of thermal runaway problems and catastrophic battery explosion accidents. The reasons are mainly the following two points: 1. The heat resistance temperature of existing silica aerogel insulation materials is generally around 600°C, but the peak temperature of thermal runaway of lithium-ion batteries can easily exceed 600°C, so the heat resistance temperature of aerogel insulation materials must be increased; 2. Aerogel insulation materials are very brittle when burned by high-temperature flames, and their insufficient mechanical strength leads to poor flame ablation resistance, making it difficult to ensure effective insulation and fire retardant time, which in turn leads to catastrophic thermal runaway of the entire battery pack.
[0004] Chinese patent CN108892470A discloses a vibration-damping and heat-insulating elastic silica aerogel sheet, wherein a coagulant is added to a solvent and stirred evenly, and then methyltrimethoxysilane and a silicon source are added, stirred evenly, a gel accelerator is added, stirred evenly again, and a sheet-like wet gel is formed by aging the gel, and then the solvent is replaced at least twice to obtain a block-like wet gel and dry it; a sheet for a thermal management system of a lithium-ion power battery of an automobile includes a vibration-damping and heat-insulating elastic silica aerogel sheet, which is used for heat insulation and vibration reduction of lithium-ion power batteries. The vibration-damping and heat-insulating elastic silica aerogel sheet prepared by the patent can only withstand a temperature of 350°C, which is difficult to provide effective thermal protection for lithium-ion batteries.
[0005] Chinese patent CN113443889A discloses a silica aerogel glass fiber felt composite sheet, thermal insulation pad product and its application for electric vehicle batteries. The preparation method of the sheet is as follows: impregnating or spraying wet glass fiber felt or glass fiber cloth with silica hydrosol or silica hydrosol modified by metal oxide; spraying glue repair hydrosol; aging and replacing water in wet gel; supercritical drying with carbon dioxide; the thermal insulation pad product includes a sheet and a package arranged around the sheet; it is applied to the insulation of parts in the battery pack of electric vehicles and between battery core modules, high-end equipment or electromechanical equipment in narrow spaces, and safety protection after fire. The silica aerogel glass fiber felt composite sheet obtained by the patent can withstand a high temperature of 800°C, but the mechanical properties under high temperature baking are relatively poor, and it is difficult to achieve a long-term fireproof and heat-insulating effect.
[0006] From the above, we can see that when aerogel insulation layer materials are used for thermal runaway protection of lithium-ion batteries, there are still problems such as insufficient heat resistance temperature and insufficient mechanical properties in high-temperature extreme environments. Therefore, the development of aerogel insulation layer materials with high temperature resistance and excellent mechanical properties at high temperatures is of great practical significance for the safe use of lithium-ion batteries. Summary of the invention
[0007] In view of the deficiencies in the above-mentioned prior art, the present invention provides an aerogel insulation layer and a preparation method thereof, so as to achieve the following invention objectives: to prepare an aerogel insulation layer material suitable for thermal protection of lithium-ion batteries, which has good high temperature resistance and excellent mechanical properties at high temperatures.
[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0009] An aerogel thermal insulation layer and a preparation method thereof, wherein the preparation method of the aerogel thermal insulation layer comprises five steps of preparing a hydrated aluminum silicate nanofiber dispersion, preparing a sol, aging replacement, drying, and heat treatment;
[0010] The following are further improvements to the above technical solution:
[0011] Step 1: Preparation of hydrated aluminum silicate nanofiber dispersion
[0012] N-methyl-2-pyrrolidone, ethylene glycol and deionized water are mixed evenly and added into a high-speed dispersing kettle, and then hydrated aluminum silicate nanofibers are added, and the dispersion rate is controlled at 5000-9000 rpm, and after strong dispersion for 4-8 hours, a hydrated aluminum silicate nanofiber dispersion is obtained;
[0013] The diameter of the hydrated aluminum silicate nanofibers is 10-70 nm and the length is 200-1000 nm;
[0014] In the hydrated aluminum silicate nanofiber dispersion, the mass ratio of N-methyl-2-pyrrolidone, ethylene glycol, deionized water, and hydrated aluminum silicate nanofiber is 5-11:1-4:100-160:10-45.
[0015] Step 2: Sol preparation
[0016] Aluminum trichloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion are added to a mixing kettle, and stirred for 20 to 35 hours at a stirring rate of 300 to 650 rpm to obtain an alumina sol. ZrOCl2·8H2O, deionized water, anhydrous ethanol, and ethyl orthosilicate are added to another reaction kettle, and then stirred for 24 to 36 hours at a stirring rate of 300 to 700 rpm to obtain a silicon dioxide and zirconium dioxide composite sol. Then, the silicon dioxide and zirconium dioxide composite sol is added to the alumina sol, and then stirred for 40 to 60 minutes at a stirring rate of 400 to 700 rpm, and then propylene oxide is added, and then the stirring rate is increased to 900 to 1200 rpm, and stirred for 30 to 50 minutes, and then the stirring is stopped, and the stirred and mixed sol is poured into a mold, and the gel is allowed to stand for 24 to 40 hours to obtain a composite gel.
[0017] In the alumina sol, the mass ratio of aluminum chloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion is 20-55:65-110:30-80:40-70;
[0018] In the silicon dioxide and zirconium dioxide composite sol, the mass ratio of ZrOCl2·8H2O, deionized water, anhydrous ethanol, and ethyl orthosilicate is 15-45:85-120:20-60:20-40;
[0019] In the composite gel, the mass ratio of the silicon dioxide and zirconium dioxide composite sol, the aluminum oxide sol and propylene oxide is 30-70:15-50:1-4.
[0020] Step 3: Aging replacement
[0021] Add an aging soaking liquid with a volume equal to that of the composite gel to the composite gel, drain the liquid after aging and soaking for 20 to 28 hours, then add an aging soaking liquid with a volume equal to that of the composite gel, drain the liquid after aging and soaking for 20 to 28 hours, then add a replacement liquid with a volume equal to that of the composite gel, soak for 24 to 36 hours, drain the liquid after draining, then add a replacement liquid with a volume equal to that of the composite gel, soak for 24 to 36 hours, to obtain an aged and replaced composite gel;
[0022] The aging soaking liquid is prepared by mixing dioxane, N,N-diethylhydroxylamine and anhydrous ethanol, wherein the mass ratio of dioxane, N,N-diethylhydroxylamine and anhydrous ethanol is 3-9:1-2.5:50-90;
[0023] The replacement fluid is prepared by mixing methyl polysilazane, 3-dimethylaminoethyl silane and n-hexane, wherein the mass ratio of methyl polysilazane, 3-dimethylaminoethyl silane and n-hexane is 5-11:0.5-2:80-120;
[0024] The number average molecular weight of the methyl polysilazane is 15000-25000 g / mol, and the viscosity at room temperature is 200-400 mPa•s.
[0025] Step 4: Drying
[0026] The aged and replaced composite gel is placed in an oven, heated at a heating rate of 0.5~1℃ / min and kept at a constant temperature of 50~65℃. After constant temperature drying for 6~9 hours, the temperature is then heated at a heating rate of 0.5~1℃ / min and kept at a constant temperature of 70~85℃. After constant temperature drying for 3~6 hours, the temperature is further heated at a heating rate of 0.5~1℃ / min and kept at a constant temperature of 110~125℃. After constant temperature drying for 2~5 hours, the temperature is cooled to room temperature to obtain a dry aerogel.
[0027] Step 5: Heat treatment
[0028] The dried aerogel is placed in a muffle furnace, heated at a heating rate of 3-6°C / min and kept at a constant temperature of 900-1000°C. After constant temperature heat treatment for 1-2.5 hours, an aerogel insulation layer is obtained.
[0029] Compared with the prior art, the present invention achieves the following beneficial effects:
[0030] 1. The present invention uses aluminum chloride, ZrOCl2·8H2O and tetraethyl orthosilicate as raw materials to prepare a ternary composite aerogel insulation layer of silicon dioxide, zirconium dioxide and aluminum oxide, and adds hydrated aluminum silicate nanofibers to strengthen and toughen the aerogel. This nano-scale aluminum silicate fiber reinforced and toughened ternary composite aerogel overcomes the limitation that the upper limit of the temperature tolerance of a single silicon dioxide aerogel can only reach 550-600°C, and increases the temperature resistance limit to more than 1000°C. Moreover, it can maintain very good mechanical properties at a high temperature of 1000°C, making it particularly suitable for thermal runaway protection of lithium-ion batteries;
[0031] 2. The present invention uses two polar organic solvents, N-methyl-2-pyrrolidone and ethylene glycol, to effectively disperse the hydrated aluminum silicate nanofibers, so that the hydrated aluminum silicate nanofibers reach a nano-scale dispersion in water. There are a lot of silanol hydroxyl groups on the surface of the hydrated aluminum silicate nanofibers, and there are very strong hydrogen bonding effects between these silanol hydroxyl groups, so that there is a very serious agglomeration phenomenon between the hydrated aluminum silicate nanofibers. After adding N-methyl-2-pyrrolidone and ethylene glycol, two polar organic solvents with hydrogen bonding adsorption effects, the surfaces of the strongly dispersed hydrated aluminum silicate nanofibers will absorb and wrap the two solvent molecules, and then the dispersed hydrated aluminum silicate nanofibers will not re-agglomerate, thus ensuring that the hydrated aluminum silicate nanofibers in the hydrated aluminum silicate nanofiber dispersion can maintain a nano-scale monodispersed state for a long time;
[0032] 3. The dioxane and N,N-diethylhydroxylamine added to the aging soaking solution of the present invention can form hydrogen bonds with the silanol groups and the terminal hydroxyl groups of the alumina sol molecular structure to control the hydrolysis rate and condensation reaction rate of each monomer in the sol and gel state, thereby inhibiting the excessive growth of gel particles and making the pore size of the gel particles and the gel network uniform. This uniform network reduces the drying stress and reduces the shrinkage during drying, so that the microstructure of the entire aerogel can be kept almost unchanged by minimizing the volume shrinkage during drying, which maximizes the strength and toughness of the overall skeleton network structure of the aerogel, so that it can still maintain extremely high mechanical properties in a high temperature environment;
[0033] 4. The present invention adds two aerogel hydrophobic modifiers, methyl polysilazane and 3-dimethylaminoethyl silane, to the displacement fluid. These two substances can make the aerogel surface have hydrophobic
[0034] Water-based, reducing the number of unreacted silanols and other polar functional groups in the gel pores, reducing irreversible shrinkage during drying. At the same time, the introduction of hydrophobic groups will also reduce the rigid connection inside the gel and increase the flexibility of the aerogel. In addition, the mutual repulsion between the hydrophobic parts also promotes the rebound during drying, which also provides favorable conditions for the subsequent atmospheric pressure drying of the aerogel, ensuring the stability of the internal network microporous structure of the aerogel during the atmospheric pressure drying process, so that the final aerogel insulation layer will have very excellent mechanical properties and high temperature resistance;
[0035] 5. The aerogel insulation layer obtained by the present invention has a thermal conductivity of 0.021~0.025mW / (m·K) at room temperature, 0.026~0.029mW / (m·K) at 400℃, 0.032~0.038mW / (m·K) at 600℃, 0.040~0.043mW / (m·K) at 800℃, and 0.046~0.049mW / (m·K) at 1000℃. The thickness shrinkage rate after baking under a 1000℃ flame for 40 minutes is 0.13~0.14%, and the mass loss rate is 0.25~0.31%. In the simulated thermal runaway test of lithium-ion batteries, the thermal runaway peak temperature is 1094~1136℃ and the cold surface temperature of the test sample is 174~191℃ within 22~26 minutes at the thermal runaway peak temperature ±200℃. DETAILED DESCRIPTION
[0036] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0037] Example 1: A method for preparing an aerogel thermal insulation layer
[0038] Step 1: Preparation of hydrated aluminum silicate nanofiber dispersion
[0039] N-methyl-2-pyrrolidone, ethylene glycol and deionized water were mixed evenly and added into a high-speed dispersing kettle, and then hydrated aluminum silicate nanofibers were added. After controlling the dispersing rate at 6500 rpm and dispersing vigorously for 7 hours, a hydrated aluminum silicate nanofiber dispersion was obtained.
[0040] The diameter of the hydrated aluminum silicate nanofibers is 50 nm and the length is 800 nm;
[0041] In the hydrated aluminum silicate nanofiber dispersion, the mass ratio of N-methyl-2-pyrrolidone, ethylene glycol, deionized water, and hydrated aluminum silicate nanofiber is 9:3:150:25.
[0042] Step 2: Sol preparation
[0043] Aluminum trichloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion were added to a mixing kettle, and stirred at a stirring rate of 550 rpm for 32 hours to obtain an alumina sol. ZrOCl2·8H2O, deionized water, anhydrous ethanol, and ethyl orthosilicate were added to another reaction kettle, and then stirred at a stirring rate of 600 rpm for 32 hours to obtain a silicon dioxide and zirconium dioxide composite sol. Then, the silicon dioxide and zirconium dioxide composite sol was added to the alumina sol, and then stirred at a stirring rate of 580 rpm for 55 minutes, and then propylene oxide was added. The stirring rate was increased to 1100 rpm, and the stirring was stopped after 45 minutes. The stirred and mixed sol was poured into a mold, and the gel was allowed to stand for 35 hours to obtain a composite gel.
[0044] In the alumina sol, the mass ratio of aluminum chloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion is 40:90:65:65;
[0045] In the silicon dioxide and zirconium dioxide composite sol, the mass ratio of ZrOCl2·8H2O, deionized water, anhydrous ethanol and ethyl orthosilicate is 35:110:45:35;
[0046] In the composite gel, the mass ratio of the silicon dioxide and zirconium dioxide composite sol, the aluminum oxide sol and propylene oxide is 55:30:2.
[0047] Step 3: Aging replacement
[0048] Add an aging soaking liquid with a volume equal to that of the composite gel to the composite gel, drain the liquid after aging and soaking for 25 hours, then add an aging soaking liquid with a volume equal to that of the composite gel, drain the liquid after aging and soaking for 25 hours, then add a replacement liquid with a volume equal to that of the composite gel, soak for 33 hours, drain the liquid, then add a replacement liquid with a volume equal to that of the composite gel, soak for 33 hours, to obtain an aged and replaced composite gel;
[0049] The aging soaking liquid is prepared by mixing dioxane, N,N-diethylhydroxylamine and anhydrous ethanol, wherein the mass ratio of dioxane, N,N-diethylhydroxylamine and anhydrous ethanol is 7:2:75;
[0050] The replacement fluid is prepared by mixing methyl polysilazane, 3-dimethylaminoethyl silane and n-hexane, wherein the mass ratio of methyl polysilazane, 3-dimethylaminoethyl silane and n-hexane is 9:1:110;
[0051] The number average molecular weight of the methyl polysilazane is 21000 g / mol, and the viscosity at room temperature is 350 mPa•s.
[0052] Step 4: Drying
[0053] The aged and replaced composite gel was placed in an oven, heated at a heating rate of 0.8°C / min and kept at a constant temperature of 60°C. After constant temperature drying for 8 hours, the temperature was then heated at a heating rate of 0.8°C / min and kept at a constant temperature of 80°C. After constant temperature drying for 4 hours, the temperature was further heated at a heating rate of 0.9°C / min and kept at a constant temperature of 119°C. After constant temperature drying for 4 hours, the temperature was cooled to room temperature to obtain a dry aerogel.
[0054] Step 5: Heat treatment
[0055] The dried aerogel was placed in a muffle furnace, and the temperature was increased at a heating rate of 4°C / min and kept constant at 980°C. After constant temperature heat treatment for 2 hours, an aerogel insulation layer was obtained.
[0056] Example 2: A method for preparing an aerogel thermal insulation layer
[0057] Step 1: Preparation of hydrated aluminum silicate nanofiber dispersion
[0058] N-methyl-2-pyrrolidone, ethylene glycol and deionized water were mixed evenly and added into a high-speed dispersing kettle, and then hydrated aluminum silicate nanofibers were added. After controlling the dispersing speed at 5000 rpm and dispersing vigorously for 4 hours, a hydrated aluminum silicate nanofiber dispersion was obtained.
[0059] The diameter of the hydrated aluminum silicate nanofibers is 10 nm and the length is 200 nm;
[0060] In the hydrated aluminum silicate nanofiber dispersion, the mass ratio of N-methyl-2-pyrrolidone, ethylene glycol, deionized water, and hydrated aluminum silicate nanofiber is 5:1:100:10.
[0061] Step 2: Sol preparation
[0062] Aluminum trichloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion are added to a mixing kettle, and stirred for 20 hours at a stirring rate of 300 rpm to obtain an alumina sol. At the same time, ZrOCl2·8H2O, deionized water, anhydrous ethanol, and ethyl orthosilicate are added to another reaction kettle, and then stirred for 24 hours at a stirring rate of 300 rpm to obtain a silicon dioxide and zirconium dioxide composite sol. Subsequently, the silicon dioxide and zirconium dioxide composite sol is added to the alumina sol, and then stirred for 40 minutes at a stirring rate of 400 rpm, and then propylene oxide is added, and then the stirring rate is increased to 900 rpm, and after stirring for 30 minutes, the stirring is stopped, and the stirred and mixed sol is poured into a mold, and after standing for 24 hours to obtain a composite gel;
[0063] In the alumina sol, the mass ratio of aluminum chloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion is 20:65:30:40;
[0064] In the silicon dioxide and zirconium dioxide composite sol, the mass ratio of ZrOCl2·8H2O, deionized water, anhydrous ethanol and ethyl orthosilicate is 15:85:20:20;
[0065] In the composite gel, the mass ratio of the silicon dioxide and zirconium dioxide composite sol, the aluminum oxide sol and propylene oxide is 30:15:1.
[0066] Step 3: Aging replacement
[0067] Add an aging soaking liquid with a volume equal to that of the composite gel to the composite gel, drain the liquid after aging and soaking for 20 hours, then add an aging soaking liquid with a volume equal to that of the composite gel, drain the liquid after aging and soaking for 20 hours, then add a replacement liquid with a volume equal to that of the composite gel, soak for 24 hours, drain the liquid after draining, then add a replacement liquid with a volume equal to that of the composite gel, soak for 24 hours, and obtain an aged and replaced composite gel;
[0068] The aging soaking liquid is prepared by mixing dioxane, N,N-diethylhydroxylamine and anhydrous ethanol, wherein the mass ratio of dioxane, N,N-diethylhydroxylamine and anhydrous ethanol is 3:1:50;
[0069] The replacement fluid is prepared by mixing methyl polysilazane, 3-dimethylaminoethyl silane and n-hexane, wherein the mass ratio of methyl polysilazane, 3-dimethylaminoethyl silane and n-hexane is 5:0.5:80;
[0070] The number average molecular weight of the methyl polysilazane is 15000 g / mol, and the viscosity at room temperature is 200 mPa•s.
[0071] Step 4: Drying
[0072] The aged and replaced composite gel was placed in an oven, heated at a heating rate of 0.5°C / min and kept at a constant temperature of 50°C. After constant temperature drying for 6 hours, the temperature was then heated at a heating rate of 0.5°C / min and kept at a constant temperature of 70°C. After constant temperature drying for 3 hours, the temperature was further heated at a heating rate of 0.5°C / min and kept at a constant temperature of 110°C. After constant temperature drying for 2 hours, the temperature was cooled to room temperature to obtain a dry aerogel.
[0073] Step 5: Heat treatment
[0074] The dried aerogel was placed in a muffle furnace, and the temperature was increased at a heating rate of 3°C / min and kept constant at 900°C. After constant temperature heat treatment for 1 hour, an aerogel insulation layer was obtained.
[0075] Example 3: A method for preparing an aerogel thermal insulation layer
[0076] Step 1: Preparation of hydrated aluminum silicate nanofiber dispersion
[0077] N-methyl-2-pyrrolidone, ethylene glycol and deionized water were mixed evenly and added into a high-speed dispersing kettle, and then hydrated aluminum silicate nanofibers were added. After controlling the dispersing rate at 9000 rpm and dispersing vigorously for 8 hours, a hydrated aluminum silicate nanofiber dispersion was obtained.
[0078] The diameter of the hydrated aluminum silicate nanofibers is 70 nm and the length is 1000 nm;
[0079] In the hydrated aluminum silicate nanofiber dispersion, the mass ratio of N-methyl-2-pyrrolidone, ethylene glycol, deionized water, and hydrated aluminum silicate nanofiber is 11:4:160:45.
[0080] Step 2: Sol preparation
[0081] Aluminum trichloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion were added to a mixing kettle, and stirred for 35 hours at a stirring rate of 650 rpm to obtain an alumina sol. ZrOCl2·8H2O, deionized water, anhydrous ethanol, and ethyl orthosilicate were added to another reaction kettle, and then stirred for 36 hours at a stirring rate of 700 rpm to obtain a silicon dioxide and zirconium dioxide composite sol. The silicon dioxide and zirconium dioxide composite sol was then added to the alumina sol, and then stirred for 60 minutes at a stirring rate of 700 rpm, and then propylene oxide was added. The stirring rate was increased to 1200 rpm, and the stirring was stopped after 50 minutes. The stirred and mixed sol was poured into a mold, and the gel was allowed to stand for 40 hours to obtain a composite gel.
[0082] In the alumina sol, the mass ratio of aluminum chloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion is 55:110:80:70;
[0083] In the silicon dioxide and zirconium dioxide composite sol, the mass ratio of ZrOCl2·8H2O, deionized water, anhydrous ethanol and ethyl orthosilicate is 45:120:60:40;
[0084] In the composite gel, the mass ratio of the silicon dioxide and zirconium dioxide composite sol, the aluminum oxide sol and propylene oxide is 70:50:4.
[0085] Step 3: Aging replacement
[0086] Add an aging soaking liquid with a volume equal to that of the composite gel to the composite gel, drain the liquid after aging and soaking for 28 hours, then add an aging soaking liquid with a volume equal to that of the composite gel, drain the liquid after aging and soaking for 28 hours, then add a replacement liquid with a volume equal to that of the composite gel, soak for 36 hours, drain the liquid, then add a replacement liquid with a volume equal to that of the composite gel, soak for 36 hours, to obtain an aged and replaced composite gel;
[0087] The aging soaking liquid is prepared by mixing dioxane, N,N-diethylhydroxylamine and anhydrous ethanol, wherein the mass ratio of dioxane, N,N-diethylhydroxylamine and anhydrous ethanol is 9:2.5:90;
[0088] The replacement fluid is prepared by mixing methyl polysilazane, 3-dimethylaminoethyl silane and n-hexane, wherein the mass ratio of methyl polysilazane, 3-dimethylaminoethyl silane and n-hexane is 11:2:120;
[0089] The number average molecular weight of the methyl polysilazane is 25000 g / mol, and the viscosity at room temperature is 400 mPa•s.
[0090] Step 4: Drying
[0091] The aged and replaced composite gel was placed in an oven, heated at a heating rate of 1°C / min and maintained at a constant temperature of 65°C. After constant temperature drying for 9 hours, the temperature was then heated at a heating rate of 1°C / min and maintained at a constant temperature of 85°C. After constant temperature drying for 6 hours, the temperature was further heated at a heating rate of 1°C / min and maintained at a constant temperature of 125°C. After constant temperature drying for 5 hours, the temperature was cooled to room temperature to obtain a dry aerogel.
[0092] Step 5: Heat treatment
[0093] The dried aerogel was placed in a muffle furnace, and the temperature was increased at a heating rate of 6°C / min and kept constant at 1000°C. After constant temperature heat treatment for 2.5 hours, an aerogel insulation layer was obtained.
[0094] Comparative Example 1: Based on Example 1, step 1, preparation of hydrated aluminum silicate nanofiber dispersion, was not performed. In step 2, preparation of sol, 65 parts of hydrated aluminum silicate nanofiber dispersion were replaced with 65 parts of deionized water. The specific operation was as follows:
[0095] Step 1, preparation of hydrated aluminum silicate nanofiber dispersion liquid is not performed;
[0096] Step 2: Sol preparation
[0097] 65 parts of hydrated aluminum silicate nanofiber dispersion were replaced by 65 parts of deionized water, and the other operations were the same as in Example 1;
[0098] The operations of steps 3, 4 and 5 are the same as those of Example 1.
[0099] Comparative Example 2: Based on Example 1, in step 1, in the preparation of the hydrated aluminum silicate nanofiber dispersion, no N-methyl-2-pyrrolidone and ethylene glycol were added, and 9 parts of N-methyl-2-pyrrolidone and 3 parts of ethylene glycol were replaced by 12 parts of deionized water in equal amounts. The specific operation was as follows:
[0100] Step 1: Preparation of hydrated aluminum silicate nanofiber dispersion
[0101] 9 parts of N-methyl-2-pyrrolidone and 3 parts of ethylene glycol were replaced by 12 parts of deionized water, and the other operations were the same as in Example 1;
[0102] The operations of steps 2, 3 and 5 are the same as those of Example 1.
[0103] Comparative Example 3: Based on Example 1, in step 3, aging replacement, no dioxane and N,N-diethylhydroxylamine are added to the aging soaking solution, and 7 parts of dioxane and 2 parts of N,N-diethylhydroxylamine are replaced by 9 parts of anhydrous ethanol in equal amounts. The specific operation is as follows:
[0104] The operations of steps 1 and 2 are the same as those of Example 1;
[0105] Step 3: Aging replacement
[0106] No dioxane or N,N-diethylhydroxylamine was added to the aging soaking solution, and 7 parts of dioxane and 2 parts of N,N-diethylhydroxylamine were replaced by 9 parts of anhydrous ethanol in equal amounts, and the other operations were the same as in Example 1;
[0107] The operations of steps 4 and 5 are the same as those of Example 1.
[0108] Comparative Example 4: Based on Example 1, in step 3, aging replacement, methylpolysilazane and 3-dimethylaminoethylsilane are not added to the replacement solution, and 9 parts of methylpolysilazane and 1 part of 3-dimethylaminoethylsilane are replaced by 10 parts of n-hexane in equal amounts. The specific operation is as follows:
[0109] The operations of steps 1 and 2 are the same as those of Example 1;
[0110] Step 3: Aging replacement
[0111] No methylpolysilazane or 3-dimethylaminoethylsilane was added to the replacement solution, and 9 parts of methylpolysilazane and 1 part of 3-dimethylaminoethylsilane were replaced by 10 parts of n-hexane in equal amounts, and the other operations were the same as in Example 1;
[0112] The operations of steps 4 and 5 are the same as those of Example 1.
[0113] Performance Test:
[0114] The following tests were performed on the aerogel insulation layers obtained in Examples 1, 2, 3 and Comparative Examples 1, 2, 3, 4:
[0115] Referring to GB / T10294-2008 and YB-4130-2005, the thermal conductivity of the aerogel insulation layer was tested at room temperature, 400℃, 600℃, 800℃ and 1000℃. After baking at 1000℃ for 40 minutes, the thickness shrinkage and mass loss rate were tested.
[0116] The thermal insulation effect of lithium-ion battery thermal runaway scenarios was simulated and tested. A quartz lamp heating table was selected to heat the battery to trigger thermal runaway. The monitoring temperature threshold of the thermocouple was 1400°C. The thermocouples were sequentially attached to the corresponding positions of the battery cell and the shell. Each thermocouple was separated by a single pack of battery cells or a piece of aerogel insulation layer to be tested. The length and width of the aerogel insulation layer to be tested were equivalent to the battery cell, and the thickness of a single piece was about 3mm. The two packs of battery cells used for the test were connected in parallel. The peak temperature of the battery cell during thermal runaway, the duration within ±200°C of the peak temperature, and the maximum value of the cold surface temperature of the aerogel insulation layer were recorded.
[0117] The specific test results are shown in Table 1:
[0118] Table 1
[0119]
[0120] From the data in Table 1, it can be seen that the thermal conductivity of Comparative Example 1 without adding hydrated aluminum silicate nanofibers is slightly lower than that of Example 1, but the thickness shrinkage rate and mass loss rate are the highest among all the embodiments and comparative examples, and the maximum value of the cold surface temperature during thermal runaway is as high as 452°C, which shows that the hydrated aluminum silicate nanofibers have an extremely slight effect on the thermal conductivity of the aerogel thermal insulation layer, but play a vital role in improving the mechanical properties and flame ablation resistance of the aerogel thermal insulation layer at high temperatures; In the preparation of the hydrated aluminum silicate nanofiber dispersion liquid of Comparative Example 2, N-methyl-2-pyrrolidone and ethylene glycol are not added. The thermal conductivity of Comparative Example 2 is significantly higher than that of Example 1, and the thickness shrinkage rate and mass loss rate as well as the maximum value of the cold surface temperature during thermal runaway are far worse than those of Example 1, which shows that the addition of N-methyl-2-pyrrolidone and ethylene glycol can effectively disperse the hydrated aluminum silicate nanofibers to obtain a nano-scale dispersion degree, thereby ensuring the strengthening and toughening effect of the hydrated aluminum silicate nanofibers on the aerogel thermal insulation layer; Comparative Example The aging immersion solution of Example 3 does not add dioxane and N,N-diethylhydroxylamine. The thermal conductivity of Comparative Example 3 is significantly higher than that of Example 1, and the thickness shrinkage rate and mass loss rate are also significantly greater than those of Example 1. The cold surface temperature during thermal runaway is also much higher than that of Example 1. This may be because dioxane and N,N-diethylhydroxylamine can adjust and control the morphological structure of the micropores inside the aerogel during the aging process, promote the formation of long-range orderly micropores, and obtain a nano-scale gel structure with a more uniform pore size, thereby improving the thermal insulation and high-temperature ablation resistance of the aerogel; Comparative Example 4 in which methylpolysilazane and 3-dimethylaminoethylsilane are not added to the replacement liquid, the thermal conductivity, thickness shrinkage rate, mass loss rate and cold surface temperature during thermal runaway are much worse than those of Example 1, and are also worse than those of Comparative Example 3, which shows that methylpolysilazane and 3-dimethylaminoethylsilane can also play a very good positive role in promoting the microstructure and microskeleton of the aerogel, and ultimately improve the thermal insulation and high-temperature flame ablation resistance of the aerogel insulation layer.
[0121] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing an aerogel thermal insulation layer, characterized in that: The preparation method of the aerogel thermal insulation layer includes five steps: preparing a hydrated aluminum silicate nanofiber dispersion, preparing a sol, aging and replacement, drying, and heat treatment; The hydrated aluminum silicate nanofiber dispersion is prepared by uniformly mixing N-methyl-2-pyrrolidone, ethylene glycol, and deionized water, adding the mixture into a high-speed dispersing kettle, and then adding the hydrated aluminum silicate nanofiber. The dispersion is controlled at a dispersion rate of 5000 to 9000 rpm and vigorously dispersed for 4 to 8 hours to obtain the hydrated aluminum silicate nanofiber dispersion. The sol is prepared by adding aluminum trichloride, deionized water, anhydrous ethanol, and a hydrated aluminum silicate nanofiber dispersion into a mixing kettle, stirring at a stirring rate of 300-650 rpm for 20-35 hours to obtain an alumina sol, and simultaneously adding ZrOCl2·8H2O, deionized water, anhydrous ethanol, and ethyl orthosilicate into another reaction kettle, stirring at a stirring rate of 300-700 rpm for 24-36 hours to obtain a silica and zirconium dioxide composite sol, then adding the silica and zirconium dioxide composite sol to the alumina sol, stirring at a stirring rate of 400-700 rpm for 40-60 minutes, adding propylene oxide, and then increasing the stirring rate to 900-1200 rpm, stirring for 30-50 minutes, stopping stirring, pouring the mixed sol into a mold, and allowing it to gel for 24-40 hours to obtain a composite gel; The aging replacement comprises adding an aging soaking liquid having a volume equal to that of the composite gel to the composite gel, aging and soaking for 20 to 28 hours, draining and draining the liquid, then adding an aging soaking liquid having a volume equal to that of the composite gel, aging and soaking for 20 to 28 hours, draining and draining the liquid, then adding a replacement liquid having a volume equal to that of the composite gel, soaking for 24 to 36 hours, draining and draining the liquid, then adding a replacement liquid having a volume equal to that of the composite gel, and soaking for 24 to 36 hours to obtain an aged and replaced composite gel; The aging soaking solution is prepared by mixing dioxane, N,N-diethylhydroxylamine, and anhydrous ethanol, wherein the mass ratio of dioxane, N,N-diethylhydroxylamine, and anhydrous ethanol is 3-9:1-2.5:50-90; The displacement fluid is prepared by mixing methylpolysilazane, 3-dimethylaminoethylsilane, and n-hexane, wherein the mass ratio of methylpolysilazane, 3-dimethylaminoethylsilane, and n-hexane is 5-11:0.5-2:80-120; The drying step comprises placing the aged and replaced composite gel in an oven, heating the temperature at a heating rate of 0.5-1°C / min and maintaining the temperature at 50-65°C, drying at the constant temperature for 6-9 hours, then heating the temperature at a heating rate of 0.5-1°C / min and maintaining the temperature at 70-85°C, drying at the constant temperature for 3-6 hours, then heating the temperature at a heating rate of 0.5-1°C / min and maintaining the temperature at 110-125°C, drying at the constant temperature for 2-5 hours, and then cooling the temperature to room temperature to obtain a dried aerogel; The heat treatment comprises placing the dried aerogel into a muffle furnace, heating the aerogel at a heating rate of 3-6°C / min and maintaining the temperature at 900-1000°C, and heat-treating the aerogel at the constant temperature for 1-2.5 hours to obtain an aerogel insulation layer.
2. The method for preparing an aerogel thermal insulation layer according to claim 1, wherein: The diameter of the hydrated aluminum silicate nanofibers is 10-70 nm and the length is 200-1000 nm; In the hydrated aluminum silicate nanofiber dispersion, the mass ratio of N-methyl-2-pyrrolidone, ethylene glycol, deionized water, and hydrated aluminum silicate nanofiber is 5-11:1-4:100-160:10-45.
3. The method for preparing an aerogel thermal insulation layer according to claim 1, wherein: In the alumina sol, the mass ratio of aluminum chloride, deionized water, anhydrous ethanol, and hydrated aluminum silicate nanofiber dispersion is 20-55:65-110:30-80:40-70; In the silicon dioxide and zirconium dioxide composite sol, the mass ratio of ZrOCl2·8H2O, deionized water, anhydrous ethanol, and ethyl orthosilicate is 15-45:85-120:20-60:20-40; In the composite gel, the mass ratio of the silicon dioxide and zirconium dioxide composite sol, the aluminum oxide sol, and propylene oxide is 30-70:15-50:1-4.
4. The method for preparing an aerogel thermal insulation layer according to claim 1, wherein: The number average molecular weight of the methyl polysilazane is 15,000-25,000 g / mol, and the viscosity at room temperature is 200-400 mPa·s.
5. The aerogel thermal insulation layer obtained by the preparation method according to any one of claims 1 to 4, characterized in that: The aerogel thermal insulation layer has a thermal conductivity of 0.021-0.025 mW / (m·K) at room temperature, 0.026-0.029 mW / (m·K) at 400°C, 0.032-0.038 mW / (m·K) at 600°C, 0.040-0.043 mW / (m·K) at 800°C, and 0.046-0.049 mW / (m·K) at 1000°C. After baking under a flame at 1000°C for 40 minutes, the aerogel thermal insulation layer has a thickness shrinkage of 0.13-0.14% and a mass loss rate of 0.25-0.31%.