Glucomannan hydrogel simulating skin extracellular matrix as well as preparation method and application of glucomannan hydrogel

By conjugating (DOPA) 4-G4-GRGDS peptide in glucomannan hydrogel to form GM-Pgdl hydrogel that simulates the skin extracellular matrix, the complex manufacturing and high cost issues in DTPI treatment are solved and achieved Healing effects without the need for other therapeutic agents, reducing inflammation and increasing tissue repair efficiency.

CN118852633AInactive Publication Date: 2024-10-29CHINA REHABILITATION SCIENCE INSTITUTE (DISABILITY PREVENTION AND CONTROL RESEARCH CENTER OF CHINA DISABLED PERSONS FEDERATION)
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410922993.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies have problems with complex manufacturing methods, uncontrolled drug release, high cost, and severe side effects when treating deep tissue pressure injury (DTPI). They are also difficult to simulate the skin extracellular matrix environment, resulting in low tissue repair efficiency.

Method used

Glucomannan hydrogel is used to form a glucomannan hydrogel that simulates the skin extracellular matrix by dynamically and acid-sensitive imine bond coupling of (DOPA)4-G4-GRGDS polypeptide and glucomannan aldehyde. (GM-Pgdl) to reduce local inflammation, promote angiogenesis and tissue repair.

Benefits of technology

GM-Pgdl hydrogel can promote the healing of DTPI without the need for other therapeutic agents, reduce local inflammation, significantly improve tissue repair efficiency, and has good biocompatibility and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852633A_ABST
    Figure CN118852633A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of biomedical materials, and particularly relates to glucomannan hydrogel simulating a skin extracellular matrix as well as a preparation method and application of the glucomannan hydrogel. The hydrogel couples a (DOPA) 4-G4-GRGDS polypeptide to the backbone of a glucomannan (GM) through a dynamic and acid sensitive imine linkage. The hydrogel simulates a glycopeptide component and a nanofiber structure of a skin extracellular matrix, creates a favorable microenvironment for proliferation and migration of cells, can reduce local inflammation of a wound, promotes angiogenesis and tissue repair, and achieves the purpose of promoting deep tissue pressure injury healing without any other therapeutic agent. Therefore, the hydrogel dressing disclosed by the invention has great clinical transformation prospects and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of biomedical materials, and in particular relates to a glucomannan hydrogel simulating skin extracellular matrix (ECM) and a preparation method and application thereof. Background Art

[0002] Deep tissue pressure injury (DTPI) is a severe manifestation of pressure injury and is more common in bedridden patients. The clinical diagnosis of DTPI is often delayed because it is difficult to tell from the appearance of the skin whether an injury has occurred in the early stages of injury. However, if left untreated, DTPI may develop into serious complications such as sepsis, renal failure, and increased mortality. The underlying mechanism of DTPI involves ischemia-reperfusion (I / R)-induced apoptosis of vascular endothelial cells and irreversible tissue damage, which establishes a proteolytic microenvironment at the wound site. This cascade reaction leads to local microcirculatory disturbances and reduced capillary density, thereby delaying the healing process. In 2018, the annual cost of DTPI treatment in the United States was reported to be $10.2 billion, which is 2.5 times the cost of ulcer prevention measures. Without effective and timely intervention, long-term infection will aggravate the damage to the local skin and deep tissues, eventually leading to chronic wounds, which will increase the suffering of patients.

[0003] Although various strategies including therapeutic drugs, cells and cytokines have been explored for immunomodulation in tissue repair, their clinical application is often hindered by challenges such as complex delivery, rapid diffusion or degradation in vivo. In recent years, hydrogel dressings have gained an important position in the field of tissue repair and regeneration. The emergence of hydrogel dressings provides a better means for tissue repair and regeneration (including wound healing), which is attributed to their three-dimensional porous network and high moisture retention ability, which can promote the exchange of oxygen and nutrients and provide a moist environment for epidermal cell migration. The latest research progress shows that drugs, cytokines or cells in hydrogels can promote wound healing. However, these methods often have problems such as complex manufacturing methods, uncontrolled drug release, high cost or large drug-related side effects.

[0004] In view of this, there is still a need to continuously explore and develop new hydrogel dressings that have good effects, simple preparation methods, low costs, and safe use, especially those that can simulate the extracellular matrix environment of the skin. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a glucomannan hydrogel capable of simulating skin extracellular matrix, and a preparation method and use thereof.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a glucomannan hydrogel simulating skin extracellular matrix, the preparation method comprising the following steps:

[0008] Step 1: Preparation of glucomannan aldehyde: Glucomannan (GM) was dissolved in double distilled water, and an aqueous sodium periodate solution was added dropwise to the reaction mixture to synthesize oxidized GM, i.e., GM-CHO;

[0009] Step 2: Preparation of glucomannan hydrogel: The GM-CHO aqueous solution prepared in step 1 is mixed with the (DOPA)4-G4-GRGDS polypeptide aqueous solution to form the glucomannan hydrogel.

[0010] As an optional manner, in the above preparation method, in step 1, the concentration of the GM aqueous solution is 1-10 wt %, and the mass volume concentration of the sodium periodate aqueous solution is 1-5%, wherein the unit of sodium periodate is g, and the unit of water is mL.

[0011] Preferably, in step 1, the concentration of the GM aqueous solution is 4 wt %, and the mass volume concentration of the sodium periodate aqueous solution is 2.14%, wherein the unit of sodium periodate is g, and the unit of water is mL.

[0012] As an optional manner, in the above preparation method, in step 1, the reaction is carried out at room temperature in a dark environment overnight and then quenched with excess ethylene glycol.

[0013] As an optional manner, in the above preparation method, in step 1, the prepared GM-CHO needs to be freeze-dried and stored in nitrogen.

[0014] As an optional mode, in the above preparation method, in step 2, the concentration of the GM-CHO aqueous solution is 1 to 10 wt %, and the concentration of the (DOPA)4-G4-GRGDS polypeptide aqueous solution is 1 to 10 wt %.

[0015] Preferably, in step 2, the concentration of the GM-CHO aqueous solution is 4 wt%, and the concentration of the (DOPA)4-G4-GRGDS polypeptide aqueous solution is 2-8 wt%.

[0016] More preferably, in step 2, the concentration of the GM-CHO aqueous solution is 4 wt %, and the concentration of the (DOPA)4-G4-GRGDS polypeptide aqueous solution is 4 wt %.

[0017] In a second aspect, the present invention provides a glucomannan hydrogel simulating skin extracellular matrix, wherein the hydrogel is prepared by the preparation method described in the first aspect.

[0018] As an optional mode, in the above glucomannan hydrogel, the hydrogel has a structure similar to the extracellular matrix of skin, and the hydrogel exhibits a high-porous network structure with a pore distribution of 3.0 to 20.0 μm.

[0019] In a third aspect, the present invention provides use of the hydrogel described in the second aspect in preparing a product for preventing or treating deep tissue pressure injury.

[0020] As an optional mode, in the above-mentioned use, the product reduces local inflammation of the wound, removes ROS, and promotes angiogenesis and tissue repair.

[0021] As an option, in the above use, the product is a functional hydrogel dressing.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The inventors have designed and developed a novel glucomannan hydrogel dressing, in which (DOPA)4-G4-GRGDS polypeptide is coupled to the backbone of glucomannan (GM) via a dynamic and acid-sensitive imine bond, denoted as GM-P gdl The hydrogel simulates the glycopeptide components and nanofiber structure of the skin extracellular matrix (ECM), creating a favorable microenvironment for cell proliferation and migration, and can reduce local inflammation of the wound, promote angiogenesis and tissue repair, and achieve the purpose of promoting DTPI healing without any other therapeutic agents. In summary, GM-P gdl Dressings have great prospects for clinical translation and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 : Glucomannan hydrogel (GM-P gdl )’s synthetic technology route.

[0025] Figure 2 :GM-P gdl Characterization. A: Hydroxylamine hydrochloride titration analysis of GM oxidation degree. Black line: sodium hydroxide titration curve. Red dotted line: first-order derivative of the titration curve; B: Gel permeation chromatography of GM (black line) and GM-CHO (red line); C: FTIR spectra of GM, GM-CHO, CAP and GM-P polymers; D: NMR spectra of GM, GM-CHO, CAP and GM-P polymers; E: GM-P used for preparation gelRepresentative images of; F: lyophilized GM-P gel Representative SEM images of .

[0026] Figure 3 :GM-P gel Rheological properties, self-healing properties, tissue adhesion and biocompatibility. A: GM-P gel Diameter distribution data of GM-P. Data represent mean ± SD (n = 3). gel Rheological analysis as a function of angular frequency (B), time (C) and shear strain (D). E: GM-P gel Self-healing properties. F: GM-P gel Macroscopic self-healing experiments were conducted. The dyes used to dye the hydrogels were rhodamine red and aniline blue. G: The hydrogel was dyed red with rhodamine dye, GM-P gel Schematic diagram of adhesion-shear tensile test. H: GM-P gel Bond shear tensile test. I: GM-P gel Representative strain-stress curves of lap shear tests with fibrin glue. J: GM-P gel Adhesion strength and interfacial toughness of GM-P gel Representative fluorescence images of L929 cells after 1, 2, and 3 days of culture. Live cells were stained with calcein-am (green); scale bar, 200 μm. L: GM-P inoculated gel Relative viability of L929 cells; M: GM-P gel The hemolysis rates of the control group and NS group were distilled water and normal saline, respectively.

[0027] Figure 4 :GM-P gel Effects on macrophage polarization, migration and tube formation. A: Use IL-4, GM-P gel (A) RAW264.7 cells were treated for 24 hours, and the expression of CD206 and CD86 was detected by flow cytometry. B and C: The percentage of M2 (B) (F4 / 80+CD206) and M1 (C) (F4 / 80+CD86) macrophages, n = 3. D: The relative mRNA expression level of IL-10. E and F: Representative images of HUVEC and quantitative analysis results of cell migration assay, n = 3. Scale bar, 100 μm. G and H: Representative images of HUVEC cell tube formation assay and quantitative analysis results. Scale bar, 100 μm.

[0028] Figure 5 :GM-P gel It can promote the healing of deep tissue injury wounds in rat skin. gelSchematic diagram of treatment of deep skin tissue injury; B: Representative images during wound healing; C: Wound surface area at different time points during wound healing; D and E: Representative images of H&E and Masson staining at 7, 14, and 21 days after treatment. F: Representative images of immunohistochemical staining for IL-6, TNF-α, and IL-10 at 21 days after treatment. Scale bar, 100 μm. DETAILED DESCRIPTION

[0029] The present invention will be further described with reference to specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention.

[0030] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0031] The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are commercially available products unless otherwise specified.

[0032] Unless otherwise specified, all percentages and parts in the present invention are percentages and parts by weight.

[0033] Example

[0034] Example 1: Glucomannan hydrogel (GM-P gel )

[0035] GM (4 wt%) was dissolved in double distilled water, and a sodium periodate aqueous solution with a mass volume concentration of 2.14% (g / mL) was added dropwise to the reaction mixture to synthesize oxidized GM, referred to as GM-CHO. The reaction was carried out at room temperature in the dark overnight and then quenched with excess ethylene glycol. The obtained GM-CHO was freeze-dried and stored in nitrogen. The glucomannan hydrogel (GM-P) of the present invention was formed by mixing the GM-CHO solution (4 wt%) with the CAP peptide solution (4 wt%). gel ).

[0036] Glucomannan hydrogel (GM-P gel )'s synthesis technology route is as follows Figure 1 shown.

[0037] Example 2: GM-P gel Characterization of hydrogels

[0038] In the present invention, inspired by the proteoglycans in the ECM, various aldehydes and hemiacetals were introduced into the backbone by oxidation with sodium periodate. Subsequently, they can react with amine groups to form imine bonds. The resulting oxidation product is called glucomannan aldehyde (GM-CHO) by colorimetric hydroxylamine titration analysis, and the degree of oxidation is 21% ( Figure 2 A). Gel permeation chromatography (GPC) analysis showed that the molecular weight of GM-CHO is comparable to that of GM ( Figure 2 B). Fourier transform infrared spectroscopy shows that the carbonyl bond is at 1642 cm- 1 There is a characteristic stretching vibration peak of an aldehyde group at Figure 2 C), confirming the successful preparation of GM-CHO.

[0039] Subsequently, GM-CHO and (DOPA)4-G4-GRGDS polypeptides were mixed in aqueous solution to mimic the glycoprotein components present in ECM to synthesize GM-P polymers (i.e., GM-Pge l Hydrogel). The chemical structure of GM-P was confirmed by nuclear magnetic resonance analysis ( Figure 2 D). The aqueous solutions of GM-CHO and (DOPA)4-G4-GRGDS peptides were combined to establish hydrogen bonds and amine bonds to synthesize GM-P mixed hydrogel (GM-Pge l ),like Figure 2 As shown in E. Figure 2 F shows that the SEM image of GM-Pge l The high-porous network structure has a pore distribution of 3.0-20.0 μm ( Figure 3 A), similar to the ECM structure.

[0040] The mechanical properties of the hybrid hydrogels were studied by dynamic rheological analysis under different mechanical conditions. Figure 3 As shown in B, at an angular frequency of 0.1 to 100 rad / s, GM-Pge l The G' (storage modulus) value always exceeds G" (loss modulus), indicating that GM-Pge l Keep it in gel form. Figure 3 Time scans in C confirmed that GM-Pge l Continuous gel state. Figure 3 D shows that both G' and G" decrease with increasing shear stress. When the strain reaches about 40%, the gel-sol phase transition occurs and G" exceeds G', indicating the injectability of the hydrogel. Figure 3 Examination of the self-healing properties of the hydrogel in E shows that at 50% strain, the moduli of G' and G" drop to lower values, indicating the presence of a sol phase. After the strain is restored to 5%, the sol state returns to the gel state, highlighting the GM-Pge l Self-healing properties.

[0041] Figure 3 F shows that qualitative estimation of the self-healing properties indicates that the separated parts of the hydrogel can automatically reunite to form a cohesive whole in the absence of external forces due to the multiple hydrogen bonds between polysaccharides. This self-healing property is believed to be essential to maintain the integrity of the hydrogel, especially considering the tendency of the skin to stretch and compress under physiological conditions.

[0042] The adhesion of hydrogel dressings to tissues is the key to effective wound closure. Figure 3 As shown in G, GM-Pge l Applied to porcine skin to evaluate its tissue adhesion ability. l It exhibits strong adhesion to pig skin and resists detachment or breakage even under repeated deformation such as stretching, twisting, bending and inversion. l The adhesion of GM-Pge survived water washing, which suggests its potential use in biofluids and dynamic environments. l The adhesion strength of the bond was quantified by lap shear test, e.g. Figure 3 H. The tensile test shows that GM-Pge l Has good shear strength and interface toughness, such as Figure 3 I and Figure 3 J. In addition, GM-Pge l The three-dimensional cross-linked network of GM-Pge is beneficial for energy dissipation during interfacial separation. l It has stable tissue adhesion, high adhesion strength, and embodies the basic properties required for wound dressings.

[0043] Example 3: GM-Pge l Biocompatibility of hydrogels

[0044] Cytocompatibility is a basic requirement for hydrogels or scaffolds in tissue engineering. Therefore, mouse fibroblast cell line L929 from ATCC was used as a model cell line, and confocal laser scanning microscopy (CLSM) was used to observe cell culture in hydrogels ( Figure 3 K). Cell viability was quantitatively determined by CCK-8 method ( Figure 3 L) The results showed that after 1, 2 and 3 days of culture, the hydrogel showed comparable cell viability to the normal cell control group (only L929 cells were inoculated) and maintained good proliferation activity. l The hemolysis rate was 4.55%, which was not significantly different from that of the sodium chloride group ( Figure 3 The above results confirm that GM-Pge l Has good biocompatibility.

[0045] Example 4: GM-Pge l It can effectively polarize macrophages to M2 type and promote cell migration and angiogenesis in vitro change

[0046] Macrophage polarization to either M1 or M2 phenotypes is often influenced by the physical and biochemical properties of biomaterials. Notably, during M2 polarization, macrophages exhibit elevated expression of the mannose receptor (MR, CD206), a C-type lectin and cell surface receptor. Given that GM is a high-affinity MR ligand, it is conceivable that GM may initiate intracellular signaling pathways associated with M2 polarization. In addition, GM-Pge l The three-dimensional nanofiber network structure is expected to provide a favorable microenvironment for cell proliferation and differentiation. l GM-Pge may regulate macrophage polarization. Using RAW264.7 cells, interleukin-4 (IL-4) was used as a positive control to evaluate the effect of GM-Pge on macrophage polarization. l Effect on polarization. Flow cytometry results ( Figure 4 A to Figure 4 C) shows that GM-Pge l Treatment increased the percentage of M2 (CD206-positive) macrophages, while the content of M1 (CD86-positive) macrophages remained low with no significant changes. In addition, IL-10, a marker of M2 macrophages, was evaluated at the mRNA level. Figure 4 In D, compared with the control cells, cells treated with GM-Pge l The treated cells showed a significant increase in the expression of IL-10 mRNA.

[0047] In addition, the effect of hydrogel on the migration of endothelial cells was detected by cell migration assay. Figure 4 E and Figure 4 The results of F showed that compared with the control group, GM-Pge l The cells in the treated group migrated more to the lower chamber, which indicated that GM-Pge l To evaluate the GM-Pge l To investigate the effect on in vitro angiogenesis, tube formation experiments were performed using Matrigel as a control. Figure 4 G and Figure 4 H display, GM-P gdl The treated group showed strong tube-forming ability, and the tube lumen formation was comparable to that of the Matrigel group. dl It not only promotes macrophage polarization to M2 type, but also promotes endothelial cell migration and angiogenesis. These effects suggest potential benefits for angiogenesis and endothelialization of damaged tissues.

[0048] Example 5: GM-P g dl Experimental study of hydrogel targeting DTPI wound healing in vivo

[0049] 1. Experimental Methods

[0050] 6-8 week old female SD rats were obtained from Beijing Weitong Lihua Experimental Animal Technology Co., Ltd. and placed in the animal barrier laboratory of the Chinese Institute of Rehabilitation Science under controlled conditions. All animal treatment procedures were ethically approved by the Institutional Animal Care and Use Committee of Capital Medical University (AEEI-2023-317). Rat model preparation The hair on the right hind limb of the SD rats was shaved, and a magnet (10 mm in diameter, 5 mm in thickness, 2.4 g in weight, 1500 G surface magnetic flux) was used to apply pressure for 12 h in the area near the superficial gluteal muscle. Within 12 hours, the rats had unlimited access to food and water and were allowed to move freely in the cage. The experimental animals were randomly divided into a control group, a chitosan treatment group, and a GM-P group. gdl Treatment groups, 5 mice in each group.

[0051] The wound site was photographed on days 3, 7, 14, and 21, and the wound area was measured using ImageJ analysis software to calculate the wound closure rate. The wound healing process was evaluated using hematoxylin and eosin (H&E) and Masson's trichrome staining. Skin specimens from the ulcer site and surrounding tissue (about 1 cm in diameter) were fixed with 10% formaldehyde solution, dehydrated, and embedded in paraffin. The skin tissue was cut into 5 μm thick sections using a microtome and stained with H&E or Masson's trichrome. Five areas were randomly selected from each section for histological analysis.

[0052] Data are presented as mean ± standard deviation (SD), and statistical significance was assessed using Student's t test or one-way analysis of variance. Significance is indicated by *p < 0.05.

[0053] 2. Experimental results

[0054] To evaluate GM-P gdl In vivo therapeutic effects of GM-P gdl As a wound dressing, a deep skin tissue injury model was established in Sprague-Dawley (SD) rats ( Figure 5 A). Chitosan was selected as a positive control due to its good regeneration ability in tissue repair. Wounds were recorded and photographed on days 3, 7, 14, and 21 after treatment. Figure 5 B and Figure 5 C shows that compared with the untreated group and the chitosan group, GM-P gdl To further verify the regeneration of skin tissue, H&E and Masson's trichrome staining were used to detect the histopathological structure of the regenerated skin during wound healing. Figure 5 D and Figure 5As shown in E, 7 days after treatment, the inflammatory cell infiltration was more severe in the control group and chitosan treatment group, while GM-Pge l The infiltration cells in the treatment group were relatively small. On day 14, the control group still had more inflammatory cell infiltration and only a small amount of collagen fibers, while GM-Pge l The dermis of the group formed regular epithelium and abundant fibroblasts. l The group showed more hair follicles, intact epidermis, and highly organized fibrillar collagen structure, in contrast, the control group and chitosan-treated group had no obvious epidermis and the collagen fibers were arranged more randomly.

[0055] Inflammation is a ubiquitous phenomenon throughout the wound healing process, which is characterized by high expression of pro-inflammatory cytokines. Figure 5 As shown in F, the secretion of IL-6 and TNF-α in the untreated wound surface was significantly increased, indicating that there were a large number of inflammatory cells in the untreated group. gel The hydrogel-treated group showed a significant decrease in the presence of IL-6 and TNF-α positive cells, suggesting that GM-P gel Reduced the expression of inflammatory cells. In addition, with GM-P gel Compared with the treatment group and chitosan hydrogel group, GM-P gel The expression of IL-10 anti-inflammatory cytokine was significantly increased in the treatment group.

[0056] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a glucomannan hydrogel simulating skin extracellular matrix, characterized in that: The preparation method comprises the following steps: Step 1: Preparation of glucomannan aldehyde: Glucomannan (GM) was dissolved in double distilled water, and an aqueous sodium periodate solution was added dropwise to the reaction mixture to synthesize oxidized GM, i.e., GM-CHO; Step 2: Preparation of glucomannan hydrogel: The GM-CHO aqueous solution prepared in step 1 is mixed with the (DOPA)4-G4-GRGDS polypeptide aqueous solution to form the glucomannan hydrogel.

2. The preparation method according to claim 1, characterized in that: In step 1, the concentration of the GM aqueous solution is 1-10 wt %, and the mass volume concentration of the sodium periodate aqueous solution is 1-5%, wherein the unit of sodium periodate is g, and the unit of water is mL.

3. The preparation method according to claim 1, characterized in that: In step 1, the reaction was carried out at room temperature in the dark overnight and then quenched with excess ethylene glycol.

4. The preparation method according to claim 1, characterized in that: In step 1, the prepared GM-CHO needs to be freeze-dried and stored in nitrogen.

5. The preparation method according to claim 1, characterized in that: In step 2, the concentration of the GM-CHO aqueous solution is 1 to 10 wt %, and the concentration of the (DOPA)4-G4-GRGDS polypeptide aqueous solution is 1 to 10 wt %.

6. A glucomannan hydrogel simulating skin extracellular matrix, characterized in that: The hydrogel is prepared by the preparation method according to any one of claims 1 to 5.

7. The glucomannan hydrogel according to claim 6, characterized in that: The hydrogel has a structure similar to that of the extracellular matrix of skin, and the hydrogel exhibits a high-pore network structure with a pore distribution of 3.0 to 20.0 μm.

8. Use of the hydrogel according to claim 6 or claim 7 in preparing a product for preventing or treating deep tissue pressure injury.

9. The use according to claim 8, characterized in that: The product reduces local inflammation of wounds, promotes angiogenesis and tissue repair.

10. The use according to claim 8, characterized in that: The product is a functional hydrogel dressing.

Citation Information

Patent Citations

  • Composite hydrogel as well as preparation method and application thereof

    CN113402733A

  • Preparation method of natural glycopeptide hydrogel

    CN118126401A

  • Implantable material comprising cellulose and the glycopeptide xyloglucan-grgds

    US20100278893A1