Mixing process of PVC composite material

By adjusting the mass ratio of PVC resin and heat stabilizer during the processing of PVC composite materials, and directly mixing the PVC resin and hot mix without hot mixing, the problems of low output and high cold water consumption of the cold mixing process are solved, and the problem is achieved. It achieves efficient cooling and good mechanical properties, reducing production costs.

CN118852809AActive Publication Date: 2024-10-29GUANGDONG LIANSU TECH INDAL
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411111540.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-29
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The cold-mixing process of PVC composite materials has a low output and requires a large amount of cold water for cooling, resulting in high production costs.

Method used

Without the need for a cooling medium, the PVC resin without hot mixing is mixed with the hot mix, and the mass ratio of the PVC resin and heat stabilizer is adjusted to achieve cooling of the hot mix, replacing the cold mixing step in the traditional process.

Benefits of technology

It increases the output of the cold mixing process, reduces energy consumption, maintains or improves the mechanical properties of PVC composite materials, and effectively reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992372960000061
    Figure BDA0004992372960000061
  • Figure BDA0004992372960000071
    Figure BDA0004992372960000071
Patent Text Reader

Abstract

The invention relates to a mixing process of a PVC composite material. The mixing process comprises the following steps: S1, preparing a hot mixture; the hot mixed material comprises the following components: PVC resin, an inorganic filler and a heat stabilizer in a mass ratio of 50: (6-10): (3-4); s2, under the condition that a cooling medium is not needed, PVC resin which is not subjected to hot mixing and the hot mixed material obtained in the step S1 are mixed. According to the mixing technology, cooling of the hot mixed material after hot mixing of the PVC composite material can be achieved under the condition that a cooling medium is not needed, the mixing energy consumption is reduced, the mixing yield is increased, and the mechanical property (compared with a traditional cold mixing technology) of the PVC composite material can be kept good or improved to some extent; therefore, the production cost of an enterprise is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PVC material processing, and more specifically to a mixing process of a PVC composite material. Background Art

[0002] PVC resin is the main material for producing pipes. In order to make the pipes have better strength, inorganic fillers (such as calcium carbonate) are usually added to the PVC composite material. In addition, since PVC resin is easy to decompose under high temperature conditions (such as hot mixing and melt extrusion) and cause material defects, heat stabilizers are usually added to PVC composite materials to prevent PVC resin from decomposing.

[0003] The processing of PVC composite materials mainly includes hot mixing-cold mixing-melt extrusion granulation, and the obtained granules are further made into pipes. Hot mixing and cold mixing are usually carried out in a hot and cold mixer. The specific process is: first, the components are put into the hot mixer according to the ratio (including PVC resin powder, fillers, additives, etc.), and the set temperature is reached after hot mixing. Then the hot mixed materials are automatically directly dropped into the cold mixer, and then the materials are cooled to a suitable temperature (usually room temperature) through the cold mixer to complete the hot mixing and cold mixing. Among them, in the hot mixing cylinder of the hot mixer, PVC resin, inorganic fillers and various additives are mixed evenly and heated to about 110 degrees Celsius. The cold mixing cylinder of the cold mixer has an interlayer in the cylinder wall, and cooling water is passed through the interlayer. The hot mixed materials are discharged into the cold mixing cylinder, and the cooling water in the interlayer of the cold mixing cylinder wall reduces the hot mixed materials to a suitable temperature.

[0004] Due to the limitations of space and production line design in actual production, the hot-mixed materials cannot be added to the extruder immediately, but need to wait for about 1 hour before adding to the extruder. This makes cold mixing play a key role in the processing of PVC composite materials.

[0005] There are three main purposes of hot mixing of PVC composite materials: first, to evenly distribute the components in space, that is, to achieve uniform mixing; second, to achieve pre-plasticization; and third, to remove as much moisture as possible from the PVC composite material. Cold mixing needs to be carried out immediately after hot mixing. The purposes of cold mixing include: first, to prevent the PVC composite material from being in a high temperature state for a long time, which may cause the PVC resin to decompose; second, to prevent the PVC composite material from reabsorbing moisture due to cooling in a natural state, thereby having a negative impact on the performance of subsequent products; third, cold mixing can further remove moisture and small molecular volatiles from the PVC composite material, and improve the mechanical properties of PVC composite products. It can be seen that in actual production, if cold mixing is not carried out, the mechanical properties of PVC composite products will be reduced due to the decomposition of PVC resin and the reabsorption of moisture.

[0006] In order to ensure the cooling effect of cold mixing, the volume of the cylinder of the cold mixer is usually more than twice that of the cylinder of the hot mixer, which limits the cold mixing output per unit time; in addition, in order to ensure the cooling effect of cold mixing, a large amount of cooling water is also required to pass through the cylinder wall of the cold mixer to assist in cooling, thereby achieving cooling of the material, but a large amount of cooling water leads to higher production costs.

[0007] If the mechanical properties of PVC composite materials can be guaranteed, the output of cold mix can be increased and the amount of cold water used can be reduced, it will bring greater benefits to the production companies. Summary of the invention

[0008] The primary purpose of the present invention is to overcome the problem that the existing cold mixing process of PVC composite materials has low output and requires a large amount of cold water for cooling, resulting in high production costs, and to provide a mixing process for PVC composite materials.

[0009] A further object of the present invention is to provide a method for preparing a PVC composite material.

[0010] The above-mentioned object of the present invention is achieved by the following technical solutions:

[0011] A mixing process for a PVC composite material comprises the following steps:

[0012] S1. Preparing a hot mix; the hot mix comprises components of a PVC resin, an inorganic filler and a heat stabilizer in a mass ratio of 50: (6 to 10): (3 to 4);

[0013] S2. Mixing the unheat-mixed PVC resin and the hot mix obtained in step S1 without the need for a cooling medium;

[0014] The mass ratio of the PVC resin that has not been hot-mixed in step S2 to the PVC resin in the hot mix is ​​1:(1.0-1.2).

[0015] The inventor of the present invention has found through many studies that by first preparing a hot mix of a certain mass ratio of PVC resin, an inorganic filler and a heat stabilizer, and then mixing it with a certain mass of PVC resin that has not been hot mixed, the PVC composite material can be reduced to a lower temperature before melt extrusion, thereby replacing the cold mixing in the traditional process. Since the cold mixing in the traditional process is not required, that is, the cooling medium (such as cold water) is not required for cooling, energy consumption is greatly saved.

[0016] The inventors of the present invention also unexpectedly discovered that by using the mixing of step S2 of the present invention instead of the cold mixing of the traditional process, the product quality (such as mechanical properties) of the PVC composite material will not decrease due to the cancellation of the cold mixing of the traditional process, but will increase relative to the quality of the PVC composite material products of the traditional process (cold mixing). The reason may be: controlling the amount of each component of the hot mix within a certain range and controlling the mass ratio of the PVC resin that has not been hot mixed to the PVC resin in the hot mix within a certain range, on the one hand, it can ensure that the temperature of the mixed material is reduced to a lower level, and on the other hand, since the PVC resin that has not been hot mixed is usually in powder or granular form, its contact with the hot mix is ​​faster and more sufficient, so that the cooling speed of the hot mix is ​​faster, the cooling uniformity is better, the decomposition of the PVC resin is less, and the consumption of the heat stabilizer is less, thereby improving the stability of the PVC composite material in subsequent processing (melt extrusion) and improving the product quality. In addition, it is also critical that the inorganic filler and the heat stabilizer are mixed with the PVC resin during the hot mixing process (step S1), which ensures the effective dispersion of the inorganic filler and the heat stabilizer in the system, which is also conducive to maintaining good mechanical properties; if some of the inorganic filler and the heat stabilizer are added in step S2, it will lead to poor mechanical properties of the material, making the use of the product risky and the company's production costs unable to be reduced.

[0017] In addition, compared with the cold mixing of the traditional process, the mixing output of step S2 of the present invention can be significantly improved, and the increase in mixing output further reduces the average energy consumption of mixing.

[0018] That is, the mixing process of the present invention can realize the cooling of the hot mixed material without the need for a cooling medium, which not only reduces the energy consumption of mixing and increases the mixing output, but also maintains or improves the mechanical properties of the PVC composite material (relative to the traditional cold mixing process), thereby effectively reducing the production cost of the enterprise.

[0019] Preferably, the inorganic filler is calcium carbonate, specifically light calcium carbonate.

[0020] Preferably, the average particle size of the inorganic filler is 2 to 10 microns.

[0021] Preferably, the heat stabilizer is a calcium zinc heat stabilizer.

[0022] Preferably, the components of the hot mix in step S1 also include other additives.

[0023] More preferably, the other additives include but are not limited to impact modifiers (eg, LB-564), lubricants (eg, YT-95), and colorants (eg, titanium dioxide).

[0024] Preferably, the process of preparing the hot mix in step S1 is: hot mixing the components of the hot mix to obtain the hot mix.

[0025] More preferably, the hot mixing time is 5 to 8 minutes and the rotation speed is 800 to 1200 r / min.

[0026] Preferably, the temperature of the hot mix in step S1 is 110-120°C.

[0027] Preferably, the mixing time in step S2 is 2 to 3 minutes, and the rotation speed is 10 to 30 r / min.

[0028] Preferably, the temperature of the PVC resin that has not been hot-mixed in step S2 is 25-30°C.

[0029] Preferably, the average polymerization degree of the PVC resin in the hot mix in step S1 or the PVC resin not hot mixed in step S2 is 300 to 1500.

[0030] Preferably, the mass ratio of the PVC resin not subjected to heat mixing in step S2 to the PVC resin in the heat mixed material is 1:(1.1-1.2). Within this mass ratio range, the impact performance of the material obtained by the mixing process is better.

[0031] Preferably, the mixing process in step S2 is carried out in a hot and cold mixer.

[0032] More preferably, the preparation of the hot mixture in step S1 is carried out in the cylinder of the hot mixer of the cold and hot mixer, and the mixing in step S2 is carried out in the cylinder of the cold mixer of the cold and hot mixer. When the mixing in step S2 is carried out in the cylinder of the cold mixer of the cold and hot mixer, the cold mixer of the cold and hot mixer does not pass the cooling medium (cooling water).

[0033] In the present invention, the cooling medium is water. That is, step S2 is: mixing the unheat-mixed PVC resin with the hot mixed material of step S1 without cooling water.

[0034] In the present invention, the hot mixed material is not cooled before the mixing in step S2. That is, in step S2, when the temperature of the hot mixed material is still 110-120°C, it is immediately mixed with the PVC resin that has not been hot mixed.

[0035] A method for preparing a PVC composite material comprises the following steps: the above-mentioned mixing process, melt extrusion and granulation to obtain the PVC composite material.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The mixing process of the present invention can realize cooling of hot mixed materials without the need for a cooling medium, which not only reduces the energy consumption of mixing and increases the mixing output, but also maintains or improves the mechanical properties of the PVC composite material (relative to the traditional cold mixing process), thereby effectively reducing the production cost of the enterprise. DETAILED DESCRIPTION

[0038] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.

[0039] Example 1

[0040] This embodiment provides a mixing process for a PVC composite material, comprising the following steps:

[0041] 1) 50 parts by weight of PVC resin (manufacturer: Zhongtai Chemical, brand: PVC-SG5), 6 parts by weight of light calcium carbonate and 4 parts by weight of heat stabilizer (BAERLOCHER MC 161FP) were added into the cylinder of a hot mixer of a 500 / 1000 cold and hot mixer, and stirred at a speed of 1000 r / min for 6 min to obtain a hot mix;

[0042] 2) The hot mixture is automatically discharged into the cylinder of the cold mixer through the 500 / 1000 hot and cold mixer. At the same time, 55 parts by weight of PVC resin (manufacturer: Zhongtai Chemical, brand: PVC-SG5, temperature: about 30°C) that has not been hot-mixed is added into the cylinder of the cold mixer of the 500 / 1000 hot and cold mixer. Without cooling water passing through the cold mixer, stirring is performed at a speed of 15 r / min for 2 minutes to complete mixing.

[0043] Example 2

[0044] This embodiment provides a mixing process of a PVC composite material, which is basically the same as that of Embodiment 1, except that:

[0045] In step 1), the amount of light calcium carbonate is 8 parts by weight and the amount of heat stabilizer is 3 parts by weight.

[0046] Example 3

[0047] This embodiment provides a mixing process of a PVC composite material, which is basically the same as that of Embodiment 1, except that:

[0048] In step 2), the amount of the PVC resin that has not been subjected to the heat mixing treatment is 50 parts by weight.

[0049] Example 4

[0050] This embodiment provides a mixing process of a PVC composite material, which is basically the same as that of Embodiment 1, except that:

[0051] In step 2), the amount of PVC resin that has not been subjected to heat mixing treatment is 60 parts by weight.

[0052] Example 5

[0053] This embodiment provides a mixing process of a PVC composite material, which is basically the same as that of Embodiment 1, except that:

[0054] In step 1), the stirring time is 4 min.

[0055] Example 6

[0056] This embodiment provides a mixing process of a PVC composite material, which is basically the same as that of Embodiment 1, except that:

[0057] In step 2), the stirring speed is 20 r / min.

[0058] Comparative Example 1

[0059] This comparative example provides a mixing process for a PVC composite material, which is basically the same as that of Example 1, except that:

[0060] In step 2), the amount of the PVC resin that has not been subjected to the heat mixing treatment is 40 parts by weight.

[0061] Comparative Example 2

[0062] This comparative example provides a mixing process for a PVC composite material, which is basically the same as that of Example 1, except that:

[0063] In step 2), the amount of the PVC resin that has not been subjected to the heat mixing treatment is 70 parts by weight.

[0064] Comparative Example 3

[0065] This comparative example provides a mixing process for a PVC composite material, which is different from Example 3 in that:

[0066] In step 1), the amounts of PVC resin, light calcium carbonate and heat stabilizer used are 50 parts by weight, 3 parts by weight and 2 parts by weight, respectively; in step 2), in addition to the hot mix and 50 parts by weight of PVC resin that has not been hot mixed, 3 parts by weight of light calcium carbonate (temperature is about 30°C) and 2 parts by weight of heat stabilizer (temperature is about 30°C) are added.

[0067] Comparative Example 4

[0068] This comparative example provides a mixing process for a PVC composite material, which is different from Example 3 in that: in step 1), the amounts of PVC resin, light calcium carbonate and heat stabilizer are 50 parts by weight, 3 parts by weight and 2 parts by weight, respectively; in step 2), no PVC resin that has not been subjected to hot mixing treatment is added, and the mixture is stirred at a speed of 15 r / min for 2 minutes while cooling water is passed through the cold mixer.

[0069] Comparative Example 5

[0070] This comparative example provides a mixing process for a PVC composite material, comprising the following steps:

[0071] 1) 50 parts by weight of PVC resin (manufacturer: Zhongtai Chemical, brand: PVC-SG5), 3 parts by weight of light calcium carbonate and 2 parts by weight of heat stabilizer (BAERLOCHER MC 161FP) were added to the cylinder of the hot mixer of a 500 / 1000 cold and hot mixer, stirred at a speed of 1000 r / min for 6 minutes to obtain a hot mix, and then placed at room temperature for 1 hour. No cold mixing was performed during the whole process.

[0072] Performance Testing

[0073] After the step 2) of the mixing process of Examples 1 to 6 and Comparative Examples 1 to 4 or the step 1) of Comparative Example 5, the materials are respectively transported to an extruder for melt extrusion and granulation, and the temperature of the melt extrusion is 160 to 210° C. to obtain a PVC composite material. The PVC composite material is injection molded into a pipe, and then its impact performance and tensile strength are tested according to GB / T14152-2016 and GB / T 8804.2-2003.

[0074] At the same time, according to the mixing process of each embodiment and comparative example, mixing was carried out continuously for 2 hours / day, and the mixing capacity (mixing amount per hour KG / hour) and energy consumption per ton of mixing (energy consumption per ton of mixing KWH / ton) of each embodiment and comparative example were calculated.

[0075] The performance test results of various embodiments and comparative examples are shown in Table 1.

[0076] Table 1

[0077]

[0078]

[0079] From Table 1, we can see that:

[0080] The materials treated by the mixing process of Examples 1 to 5 can all reach (100 / 100 without damage) in the impact performance test (equivalent to 100 samples without damage in the impact test), the tensile strength is all above 45.5 MPa, the mixing capacity is above 1590 KG / hour, and the energy consumption per ton of mixing is below 29.50 KWH / ton, indicating that the mixing process of the present invention can realize the cooling of the hot mix after the hot mixing of the PVC composite material without the need for a cooling medium, which not only reduces the mixing energy consumption and increases the mixing output, but also enables the PVC composite material to have good mechanical properties, meeting its use requirements as a pipe.

[0081] In comparative example 1, too little PVC resin without heat mixing treatment is added, resulting in poor mechanical properties of the material, wherein the result of the impact performance test of the material is 96 / 100 without breakage, indicating that there is a risk in the use of the product, and a large-scale quality inspection or waste treatment is required, thereby increasing the production cost of the enterprise. In comparative example 2, too much PVC resin without heat mixing treatment is added, resulting in poor mechanical properties of the material, wherein the result of the impact performance test of the material is 94 / 100 without breakage, indicating that there is a risk in the use of the product, and a large-scale quality inspection or waste treatment is required, thereby increasing the production cost of the enterprise. Part of the inorganic filler and heat stabilizer of comparative example 3 are added in step 2), and the mixing in step 2) cannot effectively make the inorganic filler and heat stabilizer dispersed evenly, resulting in poor mechanical properties of the material, wherein the tensile strength of the material decreases by 10.5% relative to Example 3; the result of the impact performance test of the material is 92 / 100 without breakage, indicating that there is a large risk in the use of the product, and a large-scale quality inspection or waste treatment is required, thereby increasing the production cost of the enterprise. Comparative Example 4 adopts the traditional hot mixing and cold mixing, and it can be seen that its mixing capacity is low, the average energy consumption of the mixing is high, and the tensile strength of the obtained material is obviously not as good as that of Example 3, which shows that the mixing process of the present invention can improve the mechanical properties of the material. Comparative Example 5 does not carry out the second step of the mixing process of the present invention, nor does it carry out the traditional cold mixing, but is placed at room temperature for natural cooling, resulting in significantly poor mechanical properties of the material, wherein the tensile strength of the material decreases by 12.3% relative to Example 3; the result of the impact performance test of the material is 92 / 100 without breakage, indicating that there is a great risk in the use of the product, and it needs to be subjected to large-scale quality inspection or treated as waste, thereby increasing the production cost of the enterprise; and the mixing output is low and the average energy consumption of the mixing is high.

[0082] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A mixing process for a PVC composite material, characterized in that: The steps include: S1. Preparing a hot mix; the hot mix comprises components of a PVC resin, an inorganic filler and a heat stabilizer in a mass ratio of 50: (6 to 10): (3 to 4); S2. Mixing the unheated PVC resin and the hot mix of step S1 without the need for a cooling medium; The mass ratio of the PVC resin that has not been hot-mixed in step S2 to the PVC resin in the hot mix is ​​1:(1.0-1.2).

2. The mixing process according to claim 1, characterized in that: The inorganic filler is calcium carbonate.

3. The mixing process according to claim 1, characterized in that: The heat stabilizer is a calcium zinc heat stabilizer.

4. The mixing process according to claim 1, characterized in that: The temperature of the hot mix in step S1 is 110-120°C.

5. The mixing process according to claim 1, characterized in that: The process of preparing the hot mix in step S1 is: hot mixing the components of the hot mix to obtain the hot mix.

6. The mixing process according to claim 1, characterized in that: The mixing time in step S2 is 2 to 3 minutes, and the rotation speed is 10 to 30 r / min.

7. The mixing process according to claim 1, characterized in that: The temperature of the PVC resin that has not been heat-mixed in step S2 is 25-30°C.

8. The mixing process according to claim 1, characterized in that: The average polymerization degree of the PVC resin in the hot mix in step S1 or the PVC resin not hot mixed in step S2 is 300 to 1500.

9. The mixing process according to claim 1, characterized in that: The mixing process is carried out in a hot and cold mixer.

10. A method for preparing a PVC composite material, characterized in that: The method comprises the following steps: the mixing process according to any one of claims 1 to 9, melt extrusion and granulation to obtain the PVC composite material.

Citation Information

Patent Citations

  • Rigid polyvinyl chloride (PVC-U) pipe for drinking water by using calcium-zinc stabilizer and production method thereof

    CN103554749A

  • High-reflectivity PVC (polyvinyl chloride) composite material and preparation method thereof

    CN104312043A

  • Agricultural hard thin-walled PVC tube and production process thereof

    CN105017682A

  • PVC (polyvinyl chloride) advertisement template and preparation method thereof

    CN106349606A

  • PVC thin-wall tube and production technology thereof

    CN108794934A