Durable non-stick pan coating and preparation method thereof
Through targeted selection of materials and processes, the combination of modified hexagonal boron nitride and copper sulfate solution forms a dense coating structure, which solves the problem of insufficient durability of existing non-stick pan coatings and significantly improves the bonding strength and resistance. Salt spray time.
Patent Information
- Application Number
- CN202410940083.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Existing non-stick pan coatings have shortcomings in durability and safety, lack of material fusion, and the fillers have not been modified, thus failing to take advantage of the structural strength of the coating.
Using specifically selected connecting materials and fillers, modified hexagonal boron nitride is prepared, and iron-coated hexagonal boron nitride is formed through a specific process. Combined with copper sulfate solution, the coating's binder and filler combination is improved to form Dense coating structure enhances bonding with the substrate.
It improves the tightness and environmental resistance of the coating, enhances the use effect, enables the non-stick pan to maintain good performance during long-term use, and improves the binding force and salt spray resistance.
Smart Images

Figure BDA0004943793780000081 
Figure BDA0004943793780000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating production, in particular to a durable non-stick pan coating and a preparation method thereof. Background Art
[0002] As people's living standards continue to improve, the requirements for kitchen utensils are getting higher and higher. Anti-stick coatings are widely used in daily kitchen utensils such as rice cookers, non-stick pans, range hoods and gas stoves due to their good anti-stick properties and easy cleaning, and are deeply favored by consumers.
[0003] There are many coatings for non-stick pans, but most of the current technologies focus on the use of fluorine-containing materials, which have certain shortcomings in durability and safety, and lack the targeted integration of materials. For example, the patent number CN202210934700.2 is a high-temperature wear-resistant hydrophilic inorganic coating and its preparation method and application, the coating includes component A, component B and water, wherein, by weight: component A includes: 45-75 parts of silica sol, 10-20 parts of γ-alumina, 0.5-5 parts of α-alumina, 1-5 parts of cobalt black, 0.1-5 parts of polyethylene glycol, and 0.1-5 parts of leveling agent; component B includes: 20-30 parts of titanium powder, 1-2 parts of γ-alumina, 1.2-30 parts of carbon material, and 1-5 parts of leveling agent. The high-temperature wear-resistant hydrophilic inorganic coating is formed by spraying, sintering at 500-600℃, and heat preservation to form a high-temperature wear-resistant hydrophilic inorganic coating. The materials used have not been improved in a targeted manner, resulting in certain deficiencies in fusion in actual use. For example, the patent number CN202110527260.4 is a non-stick pan coating based on an interpenetrating network structure, which is a mixture of an epoxy resin system and a polyurethane resin system in a mass ratio of 5-7:2-3; in parts by mass, the epoxy resin system includes: 30-50 parts of alicyclic epoxy compounds, 80-90 parts of glycidylamine type resins, 3-5 parts of modified carbon fibers, 2-5 parts of tetrakis (3,5-di-tert-butyl-4-hydroxyhydrocinnamic acid) pentaerythritol ester, 3-5 parts of zirconium oxide ceramics, 11-12 parts of alumina ceramics, 10-15 parts of zinc oxide ceramics, 13-17 parts of silicon nitride ceramics, and 2-5 parts of polyethylene wax; the fillers used are not modified between organic molecules, and the structural strength advantages of the coating are not brought into play. Therefore, it is extremely necessary to conduct research on deep modification of current materials to strengthen non-stick pan coatings. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the present invention provides a durable non-stick pan coating and a preparation method thereof, and strengthens the non-stick pan coating and improves its durability through targeted selection of connecting materials and fillers. The specific technical scheme is as follows:
[0005] A durable non-stick pan coating is made of the following components in parts by mass:
[0006] 8-10 parts of organic binder, 3-5 parts of silica sol, 6-9 parts of filler, 1-2 parts of modified hexagonal boron nitride, 0.1-0.3 parts of water-based bentonite, 0.1-0.2 parts of dispersant, 0.1-0.3 parts of defoamer, 5-7 parts of water;
[0007] The preparation method of the modified hexagonal boron nitride is:
[0008] (1) Potassium hydroxide and deionized water were mixed uniformly in a mass ratio of 2:3-4, and the mixture was sealed and allowed to stand for 11-14 minutes to obtain a solution A;
[0009] 1-3 parts of ferric citrate are mixed with 110-130 parts of deionized water, stirred for 4-7 minutes, and 20-30 parts of hexagonal boron nitride are added to the solution to obtain a mixed solution B; 2-6 parts of the supernatant in solution A are taken and injected into the mixed solution B, stirred for 7-10 minutes, and 2-3 parts of carrageenan are added and stirred for 30-50 minutes;
[0010] (2) centrifuging the mixed solution B, washing it with ethanol for 2-3 times, and then washing it with deionized water for 1-2 times, taking the precipitate and heating and drying it, placing the obtained dry product in a roasting furnace, roasting it at 400-430° C. for 15-20 min under oxygen flow conditions; lowering the temperature to room temperature, passing carbon monoxide, heating it at 700-710° C. for 20-30 min, and lowering the temperature to room temperature;
[0011] Mix the powder obtained in the previous step with the copper sulfate solution, heat the temperature to 33-35°C, stir for 20-30 minutes, filter, rinse the powder with deionized water 2-3 times, and dry.
[0012] Furthermore, the dispersant is BYK-161.
[0013] Furthermore, the defoaming agent is BYK-A530.
[0014] Furthermore, the organic adhesive is acrylate.
[0015] Furthermore, the filler is prepared by mixing the following raw materials: 8-10 parts of aluminum oxide, 1-2 parts of titanium dioxide, 5-7 parts of magnesium oxide, and 2-4 parts of zinc oxide.
[0016] Furthermore, the amount of carbon monoxide used is 10-15% of the mass of hexagonal boron nitride.
[0017] Furthermore, the mass ratio of the powder to the copper sulfate solution is 1:50-67.
[0018] Furthermore, the mass fraction of the copper sulfate solution is 5-6.4%.
[0019] The method for preparing the durable non-stick pan coating of the present invention comprises:
[0020] (1) Fusion of coating materials
[0021] Mix water, filler and water-based bentonite, grind with a ball mill for 2-3 hours, add organic binder, silica sol, modified hexagonal boron nitride, dispersant and defoamer, stir and grind for 50-80 minutes;
[0022] (2) Substrate preparation
[0023] Spray a dilute nitric acid solution on the spray surface of the substrate to be sprayed, clean it with ultrapure water, and then sandblast it;
[0024] (3) Coating molding
[0025] The mixed material in (1) is sprayed onto the spraying surface of the substrate in (2) at 230-250°C, and subjected to high temperature treatment at 400-420°C for 3-5 minutes.
[0026] The method for preparing a durable non-stick pan coating according to claim 9 is characterized in that the mass fraction of the dilute nitric acid solution is 0.01-0.02%; and the spraying amount is 8-10% of the mass of the substrate.
[0027] Compared with the prior art, the technical effects of the present invention are embodied in:
[0028] The durable non-stick pan coating of the present invention is matched with targeted adhesives and fillers, so that the coating has high compactness, better environmental resistance and improved use effect. In the preparation method of modified hexagonal boron nitride, potassium hydroxide and deionized water are configured into alkaline solution, ferric citrate and deionized water are mixed, and the alkaline solution is added to the mixture to form iron hydroxide precipitation, which is coated on the surface of the hexagonal boron nitride, and carrageenan is added to strengthen the adhesion in the solution, so that the iron hydroxide precipitation and the hexagonal boron nitride have better adhesion effects, and the contact between the iron hydroxide and the hexagonal boron nitride is promoted; after heating and drying, the obtained dried product is placed in a roasting furnace, and under oxygen conditions, the carrageenan is removed by roasting, and the iron hydroxide is decomposed to form iron oxide, the temperature is lowered to room temperature, carbon monoxide is introduced, and heating reduction is promoted to promote the formation of iron-coated hexagonal boron nitride; and the copper sulfate solution is mixed to perform iron-copper replacement, so that the surface of the hexagonal boron nitride is covered with iron and copper, and the binding effect of the hexagonal boron nitride in the coating is improved through the binding sites of the copper-iron particles on the surface of the hexagonal boron nitride, and the boron nitride is promoted to efficiently connect the materials to form a neatly arranged dense coating structure, improve the bonding force with the substrate, increase environmental resistance, and enable the non-stick pan to maintain good performance during long-term use. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further defined below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.
[0030] Example 1
[0031] A durable non-stick pan coating is made of the following components in parts by mass:
[0032] 8 parts of organic binder, 3 parts of silica sol, 6 parts of filler, 1 part of modified hexagonal boron nitride, 0.1 parts of water-based bentonite, 0.1 parts of dispersant, 0.1 parts of defoamer, 5 parts of water; the filler is: 8 parts of aluminum oxide, 1 part of titanium dioxide, 5 parts of magnesium oxide, 2 parts of zinc oxide; the dispersant is BYK-161; the defoamer is BYK-A530; the organic binder is acrylate;
[0033] The preparation method of the modified hexagonal boron nitride is:
[0034] (1) Potassium hydroxide and deionized water were mixed uniformly in a mass ratio of 2:3, and the mixture was sealed and allowed to stand for 11 minutes to obtain a solution A;
[0035] 1 part of ferric citrate was mixed with 110 parts of deionized water, stirred for 4 minutes, and 20 parts of hexagonal boron nitride were added to the solution to obtain a mixed solution B; 2 parts of the supernatant in solution A were taken and injected into the mixed solution B, stirred for 7 minutes, and 2 parts of carrageenan were added and stirred for 30 minutes;
[0036] (2) The mixed solution B is centrifuged, rinsed twice with ethanol, and then rinsed once with deionized water. The precipitate is heated and dried, and the obtained dry product is placed in a roasting furnace and roasted at 400°C for 15 minutes under oxygen flow conditions; the temperature is lowered to room temperature, carbon monoxide is introduced, and the mixture is heated at 700°C for 20 minutes, and the temperature is lowered to room temperature;
[0037] The amount of carbon monoxide used is 10% of the mass of hexagonal boron nitride;
[0038] (3) Mix the powder obtained in the previous step with copper sulfate solution, heat the temperature to 33°C, stir for 20 minutes, filter, rinse the powder twice with deionized water, and dry;
[0039] The mass ratio of the powder to the copper sulfate solution is 1:50; the mass fraction of the copper sulfate solution is 5%;
[0040] The preparation method of the durable non-stick pan coating is as follows:
[0041] (1) Fusion of coating materials
[0042] Mix water, filler and water-based bentonite, grind with a ball mill for 2 hours, add organic binder, silica sol, modified hexagonal boron nitride, dispersant and defoamer, stir and grind for 50 minutes;
[0043] (2) Substrate preparation
[0044] Spray a dilute nitric acid solution on the spray surface of the substrate to be sprayed, clean it with ultrapure water, and then sandblast it;
[0045] The mass fraction of the dilute nitric acid solution is 0.01%; the spraying amount is 8% of the mass of the substrate;
[0046] (3) Coating molding
[0047] The mixed material in (1) is sprayed onto the spraying surface of the substrate in (2) at 230°C and subjected to high temperature treatment at 400°C for 3 minutes.
[0048] Example 2
[0049] A durable non-stick pan coating is made of the following components in parts by mass:
[0050] 10 parts of organic binder, 5 parts of silica sol, 9 parts of filler, 2 parts of modified hexagonal boron nitride, 0.3 parts of water-based bentonite, 0.2 parts of dispersant, 0.3 parts of defoamer, 7 parts of water; the filler is mixed with the following raw materials: 10 parts of aluminum oxide, 2 parts of titanium dioxide, 7 parts of magnesium oxide, and 4 parts of zinc oxide;
[0051] The dispersant is BYK-161; the defoamer is BYK-A530; the organic binder is acrylate;
[0052] The preparation method of the modified hexagonal boron nitride is:
[0053] (1) Potassium hydroxide and deionized water were mixed uniformly in a mass ratio of 2:4, and the mixture was sealed and allowed to stand for 14 minutes to obtain a solution A;
[0054] 3 parts of ferric citrate were mixed with 130 parts of deionized water, stirred for 7 minutes, and 30 parts of hexagonal boron nitride were added to the solution to obtain a mixed solution B; 6 parts of the supernatant in solution A were taken and injected into the mixed solution B, stirred for 10 minutes, and 3 parts of carrageenan were added and stirred for 50 minutes;
[0055] (2) The mixed solution B is centrifuged, rinsed with ethanol three times, and then rinsed with deionized water twice. The precipitate is heated and dried, and the obtained dry product is placed in a roasting furnace and roasted at 430°C for 20 minutes under oxygen flow conditions; the temperature is lowered to room temperature, carbon monoxide is introduced, and the mixture is heated at 710°C for 30 minutes, and the temperature is lowered to room temperature;
[0056] The amount of carbon monoxide used is 15% of the mass of hexagonal boron nitride;
[0057] (3) Mix the powder obtained in the previous step with copper sulfate solution, heat the temperature to 35°C, stir for 30 minutes, filter, rinse the powder with deionized water three times, and dry;
[0058] The mass ratio of the powder to the copper sulfate solution is 1:50-67; the mass fraction of the copper sulfate solution is 6.4%;
[0059] The preparation method of the durable non-stick pan coating is as follows:
[0060] (1) Fusion of coating materials
[0061] Mix water, filler and water-based bentonite, grind with a ball mill for 3 hours, add organic binder, silica sol, modified hexagonal boron nitride, dispersant and defoamer, stir and grind for 80 minutes;
[0062] (2) Substrate preparation
[0063] Spray a dilute nitric acid solution on the spray surface of the substrate to be sprayed, clean it with ultrapure water, and then sandblast it;
[0064] The mass fraction of the dilute nitric acid solution is 0.02%; the spraying amount is 10% of the mass of the substrate;
[0065] (3) Coating molding
[0066] The mixed material in (1) is sprayed onto the spraying surface of the substrate in (2) at 250°C and subjected to high temperature treatment at 420°C for 5 minutes.
[0067] Example 3
[0068] A durable non-stick pan coating is made of the following components in parts by mass:
[0069] 9 parts of organic binder, 4 parts of silica sol, 7 parts of filler, 2 parts of modified hexagonal boron nitride, 0.1 parts of water-based bentonite, 0.2 parts of dispersant, 0.1 parts of defoamer, 7 parts of water; the filler is: 10 parts of aluminum oxide, 1 part of titanium dioxide, 7 parts of magnesium oxide, 2 parts of zinc oxide;
[0070] The dispersant is BYK-161; the defoamer is BYK-A530; the organic binder is acrylate;
[0071] The preparation method of the modified hexagonal boron nitride is:
[0072] (1) Potassium hydroxide and deionized water were mixed uniformly in a mass ratio of 2:3, and the mixture was sealed and allowed to stand for 14 minutes to obtain a solution A;
[0073] 1 part of ferric citrate was mixed with 130 parts of deionized water, stirred for 4 minutes, and 30 parts of hexagonal boron nitride were added to the solution to obtain a mixed solution B; 2 parts of the supernatant in solution A were taken and injected into the mixed solution B, stirred for 7 minutes, and 3 parts of carrageenan were added and stirred for 30 minutes;
[0074] (2) The mixed solution B is centrifuged, rinsed with ethanol three times, and then rinsed with deionized water twice, the precipitate is taken out and heated to dry, and the obtained dry product is placed in a roasting furnace and roasted at 400°C for 20 minutes under oxygen flow conditions; the temperature is lowered to room temperature, carbon monoxide is introduced, and the mixture is heated at 700°C for 30 minutes, and the temperature is lowered to room temperature;
[0075] The amount of carbon monoxide used is 15% of the mass of hexagonal boron nitride;
[0076] (3) Mix the powder obtained in the previous step with copper sulfate solution, heat the temperature to 33°C, stir for 30 minutes, filter, rinse the powder twice with deionized water, and dry;
[0077] The mass ratio of the powder to the copper sulfate solution is 1:67; the mass fraction of the copper sulfate solution is 5%;
[0078] The preparation method of the durable non-stick pan coating is as follows:
[0079] (1) Fusion of coating materials
[0080] Mix water, filler and water-based bentonite, grind with a ball mill for 3 hours, add organic binder, silica sol, modified hexagonal boron nitride, dispersant and defoamer, stir and grind for 50 minutes;
[0081] (2) Substrate preparation
[0082] Spray a dilute nitric acid solution on the spray surface of the substrate to be sprayed, clean it with ultrapure water, and then sandblast it;
[0083] The mass fraction of the dilute nitric acid solution is 0.02%; the spraying amount is 8% of the mass of the substrate;
[0084] (3) Coating molding
[0085] The mixed material in (1) is sprayed onto the spraying surface of the substrate in (2) at 250°C and subjected to high temperature treatment at 400°C for 3 minutes.
[0086] Contrast ratio settings:
[0087]
[0088]
[0089] Test example
[0090] According to Examples 1-3 and Comparative Examples 1-4, coatings were prepared, and the bonding strength between the coatings and the substrates was tested using the WS-2005 automatic scratch technique; each group of non-stick pans was heated to 350°C at a heating rate of 15°C / min, and the maximum number of repeated heating and cooling times under stable non-stick pan coatings was recorded; the salt spray resistance of non-stick pans was tested according to the ASTMB-177 test method. The specific results are shown in the following table:
[0091] Binding force (N) Repeated heating and cooling times (times) Salt spray resistance time (h) Example 1 26.89 6357.82 203 Example 2 27.44 6123.05 192 Example 3 28.06 6277.49 188 Comparative Example 1 21.67 5289.01 143 Comparative Example 2 22.34 5483.76 157 Comparative Example 3 24.73 5742.04 174 Comparative Example 4 23.06 5538.92 163
[0092] It can be seen from the table that the non-stick pan coating of the present invention has stronger bonding force, a high number of repeated heating times, a long salt spray resistance time, and better durability.
Claims
1. A durable non-stick pan coating, characterized in that: In parts by mass, it is made of the following components: 8-10 parts of organic binder, 3-5 parts of silica sol, 6-9 parts of filler, 1-2 parts of modified hexagonal boron nitride, 0.1-0.3 parts of water-based bentonite, 0.1-0.2 parts of dispersant, 0.1-0.3 parts of defoamer, 5-7 parts of water; The preparation method of the modified hexagonal boron nitride is: (1) Potassium hydroxide and deionized water were mixed uniformly in a mass ratio of 2:3-4, and the mixture was sealed and allowed to stand for 11-14 minutes to obtain a solution A; 1-3 parts of ferric citrate are mixed with 110-130 parts of deionized water, stirred for 4-7 minutes, and 20-30 parts of hexagonal boron nitride are added to the solution to obtain a mixed solution B; 2-6 parts of the supernatant in solution A are taken and injected into the mixed solution B, stirred for 7-10 minutes, and 2-3 parts of carrageenan are added and stirred for 30-50 minutes; (2) centrifuging the mixed solution B, washing it with ethanol for 2-3 times, and then washing it with deionized water for 1-2 times, taking the precipitate and heating and drying it, placing the obtained dry product in a roasting furnace, roasting it at 400-430° C. for 15-20 min under oxygen flow conditions; lowering the temperature to room temperature, passing carbon monoxide, heating it at 700-710° C. for 20-30 min, and lowering the temperature to room temperature; Mix the powder obtained in the previous step with the copper sulfate solution, heat the temperature to 33-35°C, stir for 20-30 minutes, filter, rinse the powder with deionized water 2-3 times, and dry.
2. The durable non-stick pan coating according to claim 1, characterized in that: The dispersant is BYK-161.
3. The durable non-stick pan coating according to claim 1, characterized in that: The defoamer is BYK-A530.
4. The durable non-stick pan coating according to claim 1, characterized in that: The organic adhesive is acrylate.
5. The durable non-stick pan coating according to claim 1, characterized in that: The filler is prepared by mixing the following raw materials: 8-10 parts of aluminum oxide, 1-2 parts of titanium dioxide, 5-7 parts of magnesium oxide, and 2-4 parts of zinc oxide.
6. The durable non-stick pan coating according to claim 1, characterized in that: The amount of carbon monoxide used is 10-15% of the mass of hexagonal boron nitride.
7. The durable non-stick pan coating according to claim 1, characterized in that: The mass ratio of the powder to the copper sulfate solution is 1:50-67.
8. The durable non-stick pan coating according to claim 1, characterized in that: The mass fraction of the copper sulfate solution is 5-6.4%.
9. A method for preparing a durable non-stick pan coating according to any one of claims 1 to 8, characterized in that: include; (1) Fusion of coating materials Mix water, filler and water-based bentonite, grind with a ball mill for 2-3 hours, add organic binder, silica sol, modified hexagonal boron nitride, dispersant and defoamer, stir and grind for 50-80 minutes; (2) Substrate preparation Spray a dilute nitric acid solution on the spray surface of the substrate to be sprayed, clean it with ultrapure water, and then sandblast it; (3) Coating molding The mixed material in (1) is sprayed onto the spraying surface of the substrate in (2) at 230-250°C, and subjected to high temperature treatment at 400-420°C for 3-5 minutes.
10. The method for preparing a durable non-stick pan coating according to claim 9, characterized in that: The mass fraction of the dilute nitric acid solution is 0.01-0.02%; the spraying amount is 8-10% of the mass of the substrate.
Citation Information
Patent Citations
Non-stick pan coating based on interpenetrating network structure and preparation method thereof
CN113337176A
High-temperature-resistant wear-resistant hydrophilic inorganic coating as well as preparation method and application thereof
CN115181438A
Hexagonal boron nitride coating as well as preparation method and application thereof
CN112521778A
In-situ synthesis carbon nanophase reinforced copper-based composite coating cookware and manufacturing method thereof
CN113621279A
"brick-mortar" layered structure corrosion-resistant phosphate composite coating, and preparation method and use therefor
WO2024056109A1