Synthetic method for spraying special texture resin

By using raw materials such as benzoic acid, salicylic acid and phenol combined with modified epoxy acrylate resin and acrylate monomers, combined with UV curing technology of photoinitiators, the complex and high-cost problems of existing special texture coatings are solved. problem, achieving stable, uniform texture effects and high adhesion.

CN118852902AActive Publication Date: 2024-10-29ZHAOQING BAOJUN CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411122727.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-29
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing special texture coatings and varnishes have complex construction techniques, high costs, short storage times, and unstable texture effects, making it difficult to achieve a uniform texture effect.

Method used

It uses raw materials such as benzoic acid, salicylic acid and phenol combined with modified epoxy acrylate resin and acrylate monomer, dissolves and evenly disperses them through solvents, adds a photoinitiator and then cures under ultraviolet light, simplifying the process and improving texture stability. sex.

Benefits of technology

A special textured resin with low cost, simple construction, stable storage and good texture effect has been realized. The adhesion reaches more than 4B to meet the needs of different substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852902A_ABST
    Figure CN118852902A_ABST
Patent Text Reader

Abstract

The invention discloses a synthesis method of resin for spraying special textures. A synthesis method of spraying special texture resin specifically comprises the following steps: dissolving 30-40 parts by mass of one or more of benzoic acid, salicylic acid and phenol in 20-40 parts by mass of a solvent, adding 25-35 parts by mass of modified epoxy acrylate resin, and stirring uniformly to obtain the spraying special texture resin. And adding 5-15 parts by mass of acrylate monomer, and uniformly dispersing to obtain the spraying special texture resin. The spraying special texture resin obtained by the synthesis method provided by the invention has the advantages of good texture forming effect, good storage stability and good adhesion to PC and PET.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the technical field of photocuring, and in particular to a method for synthesizing a spray-coated special texture resin. Background technology:

[0002] Over the past decade, UV-curable coatings and inks have developed rapidly due to their environmental protection and energy-saving advantages. However, with people's personalized requirements for product surface effects, the demand for coatings or varnishes with special texture effects is increasing. The special texture effects of coatings or varnishes are often inseparable from special base materials or additives, but the current solutions have complex construction processes and high costs. Due to the complex ingredients and short storage time, stratification and precipitation are prone to occur, and the texture effect is easily affected by batch instability, making it difficult to obtain a uniform and stable texture. Summary of the invention:

[0003] The invention solves the problems existing in the prior art and provides a method for synthesizing a spray special texture resin. The spray special texture resin obtained by the synthesis method proposed by the invention has good texture effect, good storage stability, low cost and simple construction method.

[0004] The first object of the present invention is to provide a spray special texture resin, which is prepared from the following raw materials: 30-40 parts by mass of one or more of benzoic acid, salicylic acid and phenol, 25-35 parts of modified epoxy acrylate resin, 5-15 parts of acrylate monomer and 20-40 parts of solvent.

[0005] The second object of the present invention is to provide a method for synthesizing a spray-coated special texture resin, which specifically comprises the following steps: dissolving 30-40 parts by mass of one or more of benzoic acid, salicylic acid and phenol in 20-40 parts by mass of a solvent, adding 25-35 parts by mass of a modified epoxy acrylate resin, and then adding 5-15 parts by mass of an acrylate monomer to disperse evenly to obtain a spray-coated special texture resin.

[0006] Preferably, the solvent is selected from one of ethanol, isopropanol, ethyl acetate, butyl acetate and ethylene glycol ethyl ether acetate.

[0007] Preferably, the modified epoxy acrylate resin is selected from one of the brands 700, 7182 and 7152 produced by Zhaoqing Baojun Chemical Co., Ltd.

[0008] Preferably, the acrylate monomer is selected from one or more of trimethylolpropane triacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, 1,6-hexanediol diacrylate and tripropylene glycol diacrylate.

[0009] The third object of the present invention is to provide the application of the spray-coated special texture resin in the field of photocuring.

[0010] The fourth object of the present invention is to provide a curing process for the spray-coated special texture resin, comprising the following steps: adding the spray-coated special texture resin to a photoinitiator and dispersing it evenly, and then spraying it on a substrate, and after the solvent evaporates, a regular texture appears on the substrate, and at 365nm (energy 150-300mj / cm 2 ) to cure under ultraviolet light to obtain a fixed pattern with a special texture.

[0011] Preferably, the mass ratio of the spray-coated special texture resin to the photoinitiator is 100:0.5-3.0.

[0012] Preferably, the photoinitiator is selected from one of photoinitiator TPO, photoinitiator 184, photoinitiator 1173, and photoinitiator 907.

[0013] Compared with the prior art, the present invention has the following advantages:

[0014] 1. The present invention uses one or more of benzoic acid, salicylic acid and phenol, epoxy acrylate and acrylate monomer as raw materials, which is much cheaper than the special texture agent and base material used in current special texture coatings or varnishes, and the texture is stable.

[0015] 2. The synthesis method of spraying special texture resin proposed by the present invention is to evenly disperse the raw materials at room temperature.

[0016] 3. The curing process of spraying special texture resin proposed in the present invention only needs to add a suitable photoinitiator, and a stable texture can be obtained through two steps of volatilization and illumination. The curing process is simpler and easier to control than the current process on the market.

[0017] 4. The spray-coated special texture resin proposed by the present invention has good adhesion to PC and PET substrates, and the adhesion reaches above 4B. Description of the drawings:

[0018] Figure 1 The pattern obtained in Example 1 after the sprayed special texture resin is cured;

[0019] Figure 2 The pattern obtained in Example 2 after the sprayed special texture resin is cured;

[0020] Figure 3 The pattern obtained in Example 3 after the sprayed special texture resin is cured;

[0021] Figure 4 The pattern obtained in Example 4 after the sprayed special texture resin is cured;

[0022] Figure 5 The pattern obtained in Example 5 after the sprayed special texture resin is cured;

[0023] Figure 6 This is the pattern obtained in Example 6 after the sprayed special texture resin is cured. Specific implementation method:

[0024] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.

[0025] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the field of the present technology. The modified epoxy acrylate resin proposed in the present invention is purchased from Zhaoqing Baojun Chemical Co., Ltd., with item numbers 700, 7182 or 7152.

[0026] Example 1

[0027] 30 parts by mass of phenol were dissolved in 20 parts by mass of ethanol at room temperature by stirring, and then 35 parts by mass of modified epoxy acrylate with a grade of 700 produced by Zhaoqing Baojun Chemical Co., Ltd. and 15 parts by mass of trimethylolpropane triacrylate were added and evenly dispersed to obtain a spray-coated special texture resin.

[0028] The spray-coated special texture resin obtained above was added to the photoinitiator TPO, dispersed evenly and then sprayed on the PC substrate. The mass ratio of the spray-coated special texture resin to the photoinitiator TPO was 100:3. After the solvent ethanol evaporated, recrystallization appeared on the substrate with regular texture. Under 365nm ultraviolet light (energy 150mj / cm 2 ) is cured under irradiation, and the pattern of special texture is fixed, such as Figure 1 shown.

[0029] Example 2

[0030] 35 parts by mass of phenol were dissolved in 25 parts by mass of ethanol at room temperature by stirring, and then 30 parts by mass of modified epoxy acrylate with a grade of 700 produced by Zhaoqing Baojun Chemical Co., Ltd. and 10 parts by mass of pentaerythritol triacrylate were added and dispersed evenly to obtain a spray special texture resin.

[0031] The spray-coated special texture resin obtained above was added to the photoinitiator 184, dispersed evenly and then sprayed on the PET substrate. The mass ratio of the spray-coated special texture resin to the photoinitiator 184 was 100:1. After the ethanol evaporated, the substrate was recrystallized to form a regular texture. Under 365nm ultraviolet light (energy 250mj / cm2 ) is cured under irradiation, and the pattern of special texture is fixed, such as Figure 2 shown.

[0032] Example 3

[0033] 40 parts by mass of benzoic acid were dissolved in 30 parts by mass of ethyl acetate at room temperature by stirring, and then 25 parts by mass of modified epoxy acrylate with a grade of 7182 produced by Zhaoqing Baojun Chemical Co., Ltd. and 5 parts by mass of dipentaerythritol pentaacrylate were added and evenly dispersed to obtain a spray-coated special texture resin.

[0034] The spray-coated special texture resin obtained above was added to the photoinitiator TPO, dispersed evenly and then sprayed on the PC substrate. The mass ratio of the spray-coated special texture resin to the photoinitiator TPO was 100:0.5. After the ethyl acetate evaporated, the substrate was recrystallized to form a regular texture. Under 365nm ultraviolet light (energy 300mj / cm 2 ) is cured under irradiation, and the pattern of special texture is fixed, such as Figure 3 shown.

[0035] Example 4

[0036] 35 parts by mass of benzoic acid were dissolved in 25 parts by mass of butyl acetate under stirring at room temperature, and then 30 parts by mass of modified epoxy acrylate with a brand number of 7182 produced by Zhaoqing Baojun Chemical Co., Ltd. and 10 parts by mass of dipentaerythritol hexaacrylate were added and evenly dispersed to obtain a spray-coated special texture resin.

[0037] The spray-coated special texture resin obtained above was added with photoinitiator 1173, and 1 part by mass of pink color concentrate was added, dispersed evenly, and then sprayed on the PET substrate. The mass ratio of the spray-coated special texture resin to the photoinitiator 1173 was 100:1. After the butyl acetate volatilized, the substrate was recrystallized to form a regular texture. Under 365nm ultraviolet light (energy 300mj / cm 2 ) is cured under irradiation, and the pattern of special texture is fixed, such as Figure 4 shown.

[0038] Example 5

[0039] 30 parts by mass of phenol were dissolved in 40 parts by mass of ethylene glycol ethyl ether acetate at room temperature by stirring, and then 25 parts by mass of modified epoxy acrylate with a grade of 7152 produced by Zhaoqing Baojun Chemical Co., Ltd. and 5 parts by mass of 1,6-hexanediol diacrylate were added and evenly dispersed to obtain a spray-coated special texture resin.

[0040] The spray-coated special texture resin obtained above was added to the photoinitiator 907, dispersed evenly and then sprayed on the PC substrate. The mass ratio of the spray-coated special texture resin to the photoinitiator 1173 was 100:2. After the ethylene glycol ethyl ether acetate volatilized, regular textures appeared on the substrate after recrystallization. Under 365nm ultraviolet light (energy 200mj / cm 2 ) is cured under irradiation, and the pattern of special texture is fixed, such as Figure 5 shown.

[0041] Example 6

[0042] 35 parts by mass of phenol were dissolved in 25 parts by mass of isopropanol at room temperature by stirring, and then 30 parts by mass of modified epoxy acrylate with a grade of 7152 produced by Zhaoqing Baojun Chemical Co., Ltd. and 10 parts by mass of tripropylene glycol diacrylate were added and dispersed evenly to obtain a spray-coated special texture resin.

[0043] The spray-coated special texture resin obtained above was added to the photoinitiator 184, dispersed evenly and then sprayed on the PET substrate. The mass ratio of the spray-coated special texture resin to the photoinitiator 184 was 100:3. After the isopropanol evaporated, the substrate was recrystallized to form a regular texture. Under 365nm ultraviolet light (energy 150mj / cm 2 ) is cured under irradiation, and the pattern of special texture is fixed, such as Figure 6 As shown (sprayed on a bottle-shaped PET substrate). Comparing the effect of patterning, the pattern of benzoic acid is fine, the pattern of phenol is medium, and the pattern of salicylic acid is coarse. Different colors of patterns can be adjusted by adding different color concentrates to meet different needs.

[0044] The sprayed resin was sprayed onto PC and PET substrates according to the paint film formula listed in each embodiment. After the solvent evaporated, it was UV-cured and tested for adhesion. The data are shown in Table 1:

[0045] Table 1 Adhesion data of Examples 1-6

[0046] Group Adhesion to substrate (PC) Adhesion to substrate (PET) Example 1 5B 4B Example 2 5B 4B Example 3 5B 4B Example 4 5B 4B Example 5 5B 4B Example 6 5B 4B

[0047] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A spraying special texture resin, characterized in that, The invention is prepared from the following raw materials: by weight, 30-40 parts of one or more of benzoic acid, salicylic acid and phenol, 25-35 parts of modified epoxy acrylate resin, 5-15 parts of acrylate monomer and 20-40 parts of solvent.

2. A method for synthesizing a spray-coated special texture resin, characterized in that: Specifically, the method comprises the following steps: dissolving 30-40 parts by weight of one or more of benzoic acid, salicylic acid and phenol in 20-40 parts by weight of a solvent, adding 25-35 parts by weight of a modified epoxy acrylate resin, and then adding 5-15 parts by weight of an acrylate monomer and dispersing the resin uniformly to obtain a sprayable special texture resin.

3. The method for synthesizing a spray-coated special texture resin according to claim 2, characterized in that: The solvent is selected from one of ethanol, isopropanol, ethyl acetate, butyl acetate and ethylene glycol ethyl ether acetate.

4. The method for synthesizing a spray-coated special texture resin according to claim 2, characterized in that: The modified epoxy acrylate resin is selected from one of the brands 700, 7182 and 7152 produced by Zhaoqing Baojun Chemical Co., Ltd.

5. The method for synthesizing a spray-coated special texture resin according to claim 2, characterized in that: The acrylate monomer is selected from one or more of trimethylolpropane triacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, 1,6-hexanediol diacrylate and tripropylene glycol diacrylate.

6. Application of the spray-coated special texture resin according to claim 1 in the field of photocuring.

7. The curing process of spraying special texture resin according to claim 1, characterized in that: The method comprises the following steps: adding a photoinitiator to the spray-coated special texture resin described in claim 1 and dispersing the resin uniformly, spraying the resin onto a substrate, and allowing the substrate to have regular textures after the solvent evaporates, and curing the substrate under 365nm ultraviolet light to obtain a fixed pattern with special textures.

8. The curing process according to claim 7, characterized in that: The mass ratio of the spraying special texture resin to the photoinitiator is 100:0.5-3.

0.

9. The curing process according to claim 7 or 8, characterized in that: The photoinitiator is selected from one of photoinitiator TPO, photoinitiator 184, photoinitiator 1173 and photoinitiator 907.

Citation Information

Patent Citations

  • Matte PET film for decorative sheet and preparation method thereof

    CN111234283A

  • Transparent ball inner coating feather paint and preparation method thereof

    CN114806287A

  • High-adhesion UV (ultraviolet) coating on PET (polyethylene terephthalate) film, preparation method of high-adhesion UV coating and preparation method of film material

    CN115991954A

  • Method for manufacturing texture steel sheet using UV radiation coating and texture steel sheet menufactured with the method

    KR101271981B1