Visible light Fenton-chemical mechanical polishing solution for SiC, preparation method and polishing method

By using titanium-based metal organic framework MIL-125 (Ti) and visible light source irradiation in SiC surface polishing liquid, H2O2 is catalyzed to produce efficient *OH, which solves the problems of low oxidation potential and short *OH life in SiC surface polishing liquid. Efficient SiC surface polishing and environmentally friendly polishing fluid system are achieved.

CN118852984APending Publication Date: 2024-10-29HANGZHOU DIANZI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410848316.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The oxidation potential of H2O2 in the existing SiC surface polishing liquid is low, resulting in poor oxidation effect. After the catalyst is introduced, the *OH life is short and difficult to use efficiently, which limits the efficiency and quality of SiC surface polishing.

Method used

The titanium-based metal organic framework MIL-125 (Ti) is used as the Fenton catalyst, supplemented by visible light source irradiation, to efficiently catalyze H2O2 to produce a large amount of *OH with exceeding high redox potential, achieving in-situ generation and efficient utilization of *OH , to avoid *OH quenching.

Benefits of technology

It significantly increases the concentration and utilization rate of *OH, improves SiC surface polishing efficiency, reduces surface defects, meets the quality requirements for efficient SiC surface polishing, avoids the use of highly toxic components in traditional polishing solutions, and protects the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852984A_ABST
    Figure CN118852984A_ABST
Patent Text Reader

Abstract

The invention discloses a visible light Fenton-chemical mechanical polishing solution for SiC, a preparation method and a polishing method. The polishing solution comprises the following components in percentage by weight: 0.02 wt%-0.1 wt% of MIL-125 (Ti), 1 wt%-5 wt% of hydrogen peroxide, 15 wt%-30 wt% of a grinding material, 0.1 wt%-0.5 wt% of sodium carbonate, 0.1 wt%-0.5 wt% of a dispersing agent and the balance of deionized water. According to the method, MIL-125 (Ti) is adopted and assisted by irradiation of the visible light source, H2O2 can be efficiently catalyzed to generate a large amount of * OH with the potential exceeding the high oxidation-reduction potential, so that in-situ generation of * OH and efficient oxidation of SiC are achieved, the generated * OH cannot be quenched, the utilization rate of * OH can be greatly increased, and the method has the advantages of being high in polishing efficiency, few in surface defect and the like; and the SiC surface polishing quality requirement is effectively met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chemical mechanical polishing, and more specifically, to a visible light Fenton-chemical mechanical polishing liquid for SiC, a preparation method and a polishing method. Background Art

[0002] With the rapid development of new communication technologies, higher and higher requirements are placed on the research and development and manufacturing of semiconductor devices. As a third-generation semiconductor material, single-crystal SiC has the characteristics of large bandgap width, high saturated electron drift velocity, high breakdown electric field strength, high thermal conductivity, etc. It can be used under extreme conditions such as high temperature, high power, and strong radiation. It is one of the most promising semiconductor materials and has been widely used in many fields. When SiC wafers are used for epitaxial film growth, the surface is required to be ultra-smooth, free of defects and damage, and the surface roughness is less than 0.5nm. However, due to the high hardness (Mohs hardness 9.2), high brittleness and very stable chemical properties of single-crystal SiC, whether it is used as a substrate or a power device, its surface is extremely difficult to be efficiently flattened globally, and it is difficult to take into account both efficient and high-precision flattening, which greatly limits the application of SiC-based power chips and devices.

[0003] Chemical mechanical polishing (CMP) is widely used in global planarization processing of components such as single crystal silicon, quartz, and metal, and has also been successfully applied to the surface planarization of SiC substrates. CMP realizes the polishing of the object surface based on the alternating process of chemical corrosion and mechanical grinding. Its chemical corrosion rate directly affects the CMP polishing efficiency and polishing quality of the SiC surface. As the carrier for implementing CMP, the polishing liquid has a decisive influence on the polishing quality and polishing efficiency. Traditional polishing liquids often contain highly toxic strong oxidants, strong acids, strong bases and other components, which are not in line with the national green development strategy. As a result, green and environmentally friendly chemical mechanical polishing liquids have gradually developed in recent years. Among them, the most important strategy is to replace traditional toxic components with new low-toxic or non-toxic oxidants, acids / bases.

[0004] At present, it is relatively mature to use the oxidant H2O2 to replace the traditional highly toxic nitric acid, periodate, persulfate, hypochlorite, etc. For example, Chinese patents CN115124927A, CN117305843A, CN117328068A, and CN117987011A all prefer H2O2 as a green oxidant for chemical mechanical polishing. However, the oxidation potential of H2O2 is only 1.76eV, which has limited corrosion ability to the polishing object compared with traditional oxidants, and it is very easy to decompose into oxygen and water during the polishing process, resulting in low oxidation effect.

[0005] To this end, people introduced Fenton catalysts into chemical mechanical polishing liquids and used the Fenton reaction to catalyze H2O2 to achieve an ultra-high redox potential of 2.8eV, thereby improving oxidation efficiency. Among them, iron-based compounds are the most common Fenton catalysts. For example, Xu Shaoping et al. reported the CMP effects of various iron-based Fenton catalysts in the non-patent literature "Study on Solid-Phase Catalysts for Single Crystal SiC Chemical Mechanical Polishing Liquids". However, due to the fact that the H2O2 in the polishing liquid decomposes immediately when the catalyst is introduced, the generated *OH has a limited lifespan and is quenched in large quantities when entering the polishing equipment, making it difficult to efficiently utilize *OH, resulting in limited improvement in polishing efficiency. Summary of the invention

[0006] The purpose of the present invention is to overcome the above-mentioned defects of the prior art and provide a visible light Fenton-chemical mechanical polishing liquid, a preparation method and a polishing method for SiC. By adopting a titanium-based metal organic framework MIL-125 (Ti) and supplemented by visible light source irradiation, H2O2 can be efficiently catalyzed to produce a large amount of *OH with a high redox potential, thereby realizing the in-situ generation of *OH and high-efficiency oxidation of SiC. The generated *OH will not be quenched, which can greatly improve the utilization rate of *OH. It has the advantages of high polishing efficiency and few surface defects, and effectively meets the SiC surface polishing quality requirements.

[0007] To achieve the above object, the technical solution of the present invention is as follows:

[0008] A visible light Fenton-chemical mechanical polishing liquid for SiC comprises the following components in weight percentage: 0.02wt% to 0.1wt% of MIL-125 (Ti), 1wt% to 5wt% of hydrogen peroxide, 15wt% to 30wt% of abrasive, 0.1wt% to 0.5wt% of sodium carbonate, 0.1wt% to 0.5wt% of a dispersant and the balance is deionized water.

[0009] The present invention also discloses a method for preparing the visible light Fenton-chemical mechanical polishing solution for SiC as described above, comprising the following steps:

[0010] Dissolving a dispersant in deionized water, adding an abrasive and mixing the water to obtain a first suspension;

[0011] Under yellow light, adding MIL-125(Ti) and sodium carbonate into the first suspension and mixing them to obtain a second suspension;

[0012] Under yellow light, hydrogen peroxide is added to the second suspension and then mixed in the dark to obtain a visible light Fenton-chemical mechanical polishing solution.

[0013] The present invention also discloses a visible light Fenton-chemical mechanical polishing liquid as described above, or a polishing method of the visible light Fenton-chemical mechanical polishing liquid prepared by the preparation method as described above, comprising the following steps:

[0014] S1. Injecting the visible light Fenton-chemical mechanical polishing solution between the polishing pad and the SiC at room temperature, and keeping the visible light Fenton-chemical mechanical polishing solution in a dark environment throughout the process;

[0015] S2. Under the irradiation of a visible light source, the SiC is subjected to visible light Fenton-chemical mechanical polishing, and after the polishing is completed, the SiC is cleaned and dried to obtain a treated SiC.

[0016] Implementing the embodiments of the present invention will have the following beneficial effects:

[0017] (1) The present invention takes the polishing liquid that improves the in-situ generation of *OH and improves the utilization rate of *OH as the design starting point, and develops a polishing liquid system that is superior to the traditional one. By adopting a titanium-based metal organic framework and supplemented by visible light source irradiation, it can efficiently catalyze H2O2 to produce a large amount of *OH with a high redox potential, thereby achieving the in-situ generation of *OH and high-efficiency oxidation of SiC; further, the polishing liquid of the present invention is irradiated by a visible light source, and the polishing pressure, polishing liquid flow, polishing speed, visible light power and other parameters are controlled during the polishing process. It can be irradiated while polishing, and the generated *OH will not be quenched, which can greatly improve the utilization rate of *OH. Therefore, the present invention improves the concentration and utilization rate of *OH, so that when polishing SiC, it has a higher *OH to react with the workpiece for oxidation, accelerates the removal of SiC surface materials by abrasives during the polishing process, can effectively improve the polishing efficiency of SiC, has the advantages of high polishing efficiency, few surface defects, and easy cleaning of the silicon wafer surface after polishing, and effectively meets the quality requirements of SiC surface polishing.

[0018] (2) The components in the visible light Fenton-chemical mechanical polishing liquid of the present invention are green and environmentally friendly components, which effectively abandon the use of highly toxic nitric acid, periodate, persulfate, and hypochlorite in traditional polishing liquids, protect experimental equipment and the ecological environment, and after polishing, the abrasive and MIL-125 (Ti) can be separated by filtering or centrifugation, and can be reused after cleaning. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a scanning electron microscope image of the titanium-based metal organic framework MIL-125 (Ti) of Example 1 of the present invention.

[0020] Figure 2 Polarization curve test results of SiC samples of the polishing liquids of Example 1 and Comparative Examples 1-2 are shown. DETAILED DESCRIPTION

[0021] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited in any way.

[0022] The invention discloses a visible light Fenton-chemical mechanical polishing liquid for SiC, comprising the following components in weight percentage: 0.02wt% to 0.1wt% of MIL-125 (Ti), 1% to 5% of hydrogen peroxide, 15wt% to 30wt% of abrasive, 0.1wt% to 0.5wt% of sodium carbonate, 0.1wt% to 0.5wt% of a dispersant and the balance being deionized water.

[0023] Specifically, the present invention reasonably improves the composition and ratio of the polishing liquid through multiple experiments, and utilizes the synergistic effect of each component to increase the concentration and utilization rate of *OH, which is beneficial to further enhance the polishing efficiency and improve the surface quality of SiC; and the polishing liquid of the present invention avoids the use of highly toxic components such as nitric acid, periodate, persulfate, hypochlorite, etc., thereby protecting experimental equipment and the ecological environment.

[0024] In a specific embodiment, the particle size of MIL-125(Ti) is 200 nm to 500 nm.

[0025] In a specific embodiment, the particle size of MIL-125 (Ti) includes but is not limited to 200 nm, 300 nm, 400 nm, 500 nm, etc.

[0026] In a specific embodiment, the abrasive includes one or both of silicon dioxide and cerium oxide.

[0027] Preferably, the abrasive is silicon dioxide and cerium oxide. Specifically, the present invention uses composite abrasive particles to achieve mutual complementarity and mutual benefit, and can effectively avoid scratches while achieving a high polishing rate.

[0028] In a specific embodiment, the weight ratio of silicon dioxide to cerium oxide is (2-10):1.

[0029] In a specific embodiment, the particle size of the abrasive is 100nm to 500nm. Specifically, if the particle size of the abrasive is too small, the polishing rate will be reduced, and if it is too large, the surface quality of the silicon wafer will deteriorate. Therefore, the present invention can control the particle size of the abrasive to increase the removal rate and ensure good surface quality, thereby achieving efficient polishing.

[0030] In a specific embodiment, the dispersant includes one or more of sodium carboxymethyl cellulose, sodium hydroxymethyl cellulose, and polyvinyl pyrrolidone.

[0031] The present invention also discloses a method for preparing a visible light Fenton-chemical mechanical polishing solution for SiC according to any embodiment of the present invention, comprising the following steps:

[0032] S1. Dissolving a dispersant in deionized water, adding an abrasive and mixing the mixture to obtain a first suspension.

[0033] In a specific embodiment, the mixing specifically includes: ultrasonication at room temperature for 30 minutes to 60 minutes, and then stirring for 4 hours to 6 hours.

[0034] S2. Under yellow light, add MIL-125(Ti) and sodium carbonate into the first suspension and mix them to obtain a second suspension.

[0035] In a specific embodiment, the mixing is specifically ultrasonicated for 1 min to 2 min.

[0036] S3. Under yellow light, hydrogen peroxide is added to the second suspension and then mixed in the dark to obtain a visible light Fenton-chemical mechanical polishing solution.

[0037] In a specific embodiment, the present invention can separate the abrasive and MIL-125 (Ti) by filtering or centrifuging, and the abrasive and MIL-125 (Ti) can be reused after cleaning.

[0038] In a specific embodiment, the mixing is stirring for 2 min to 5 min.

[0039] In a specific embodiment, the prepared polishing liquid is stored away from light.

[0040] Specifically, the preparation method of the present invention has simple steps and is easy to operate.

[0041] The present invention also discloses a visible light Fenton-chemical mechanical polishing liquid according to any embodiment of the present invention, or a polishing method of the visible light Fenton-chemical mechanical polishing liquid prepared by the preparation method according to any embodiment of the present invention, comprising the following steps:

[0042] S1. Inject the visible light Fenton-chemical mechanical polishing solution between the polishing pad and the SiC at a flow rate of 1 mL / min to 5 mL / min at room temperature, and keep the visible light Fenton-chemical mechanical polishing solution in a dark environment during the process.

[0043] S2. Under the irradiation of a visible light source, the SiC is subjected to visible light Fenton-chemical mechanical polishing, and after the polishing is completed, the SiC is cleaned and dried to obtain a treated SiC.

[0044] In one embodiment, the polishing liquid may be continuously injected via a peristaltic pump.

[0045] In a specific embodiment, during the visible light Fenton-chemical mechanical polishing process, the rotation speed of the polishing pad is controlled to be 200rpm~1000rpm, and the polishing time is 120min~600min; the material of the polishing pad is damping cloth; the power of the visible light source is 50W~200W; and the polishing pressure is 1MPa~10MPa.

[0046] Specifically, the polishing liquid of the present invention contains MIL-125 (Ti), which can decompose H2O2 into *OH by irradiating with a visible light source and controlling parameters such as polishing pressure, polishing liquid flow, polishing speed, and visible light power during the polishing process. Polishing and irradiation can be performed simultaneously, and the generated *OH will not be quenched, which can greatly improve the utilization rate of *OH, thereby more effectively removing the oxide layer.

[0047] Specifically, the polishing liquid of the present invention can increase the concentration of *OH and its utilization rate, so that when polishing SiC, it has higher *OH to react with the workpiece for oxidation, accelerate the removal of SiC surface materials by abrasives during the polishing process, can effectively improve the polishing efficiency of SiC, and improve the surface quality, can better meet mass production needs, has low processing costs, and overcomes the problems of premature generation and extremely low utilization rate of *OH in traditional iron-based Fenton-chemical mechanical polishing liquids.

[0048] The following are specific embodiments

[0049] Example 1

[0050] The visible light Fenton-chemical mechanical polishing liquid of this embodiment includes the following components in weight percentage: 0.02wt% of MIL-125 (Ti) (particle size is 200nm), 1wt% of hydrogen peroxide, 15wt% of silica abrasive (particle size is 100nm), 0.1wt% of sodium carbonate, 0.1wt% of sodium carboxymethyl cellulose and the balance is deionized water.

[0051] The polishing method of this embodiment includes: the polishing sample is the Si surface of the SiC crystal, with a size of 2cm*2cm. The SiC sample is fixed on a UNIPOL-1200S chemical mechanical polishing device, a damping cloth is used as a polishing pad, the polishing pressure is set to 0.1MPa, and the speed is set to 200rpm. At room temperature, the above-mentioned polishing liquid is continuously stirred on the agitator for 10 minutes, and the peristaltic pump is turned on to continuously inject the polishing liquid into the polishing equipment at a flow rate of 5mL / min, and the polishing liquid device is always kept in the dark. Turn on the visible light source on the polishing equipment, the light source power is 50W, and the polishing liquid in the polishing disk is irradiated. After polishing, remove the SiC sample, rinse it thoroughly with deionized water, and blow it dry.

[0052] Example 2

[0053] The visible light Fenton-chemical mechanical polishing liquid of this embodiment includes the following components in weight percentage: 0.04wt% of MIL-125 (Ti) (particle size is 300nm), 2wt% of hydrogen peroxide, 20wt% of cerium oxide abrasive (particle size is 200nm), 0.2wt% of sodium carbonate, 0.2wt% of sodium hydroxymethyl cellulose and the balance is deionized water.

[0054] The polishing method of this embodiment is the same as that of embodiment 1.

[0055] Example 3

[0056] The visible light Fenton-chemical mechanical polishing liquid of this embodiment includes the following components in weight percentage: 0.06wt% of MIL-125 (Ti) (particle size is 400nm), 3wt% of hydrogen peroxide, 10wt% of silica abrasive (particle size is 300nm), 10wt% of cerium oxide abrasive (particle size is 500nm), 0.3wt% of sodium carbonate, 0.3wt% of polyvinyl pyrrolidone and the balance is deionized water.

[0057] The polishing method of this embodiment 1 is the same as that of embodiment 1.

[0058] Example 4

[0059] The visible light Fenton-chemical mechanical polishing liquid of this embodiment includes the following components in weight percentage: 0.08wt% of MIL-125 (Ti) (particle size is 500nm), 4wt% of hydrogen peroxide, 15wt% of silica abrasive (particle size is 500nm), 10wt% of cerium oxide abrasive (particle size is 200nm), 0.4wt% of sodium carbonate, 0.2wt% of sodium carboxymethyl cellulose, 0.2wt% of polyvinyl pyrrolidone, and the balance is deionized water.

[0060] The polishing method of this embodiment is the same as that of embodiment 1.

[0061] Example 5

[0062] The visible light Fenton-chemical mechanical polishing liquid of this embodiment includes the following components in weight percentage: 0.1wt% of MIL-125 (Ti) (particle size is 500nm), 5wt% of hydrogen peroxide, 15wt% of silica abrasive (particle size is 500nm), 15wt% of cerium oxide abrasive (particle size is 200nm), 0.5wt% of sodium carbonate, 0.3wt% of sodium carboxymethyl cellulose, 0.2wt% of polyvinyl pyrrolidone, and the balance is deionized water.

[0063] The polishing method of this embodiment is the same as that of embodiment 1.

[0064] Comparative Example 1

[0065] The only difference between this comparative example and Example 1 is that no MIL-125 (Ti) is added.

[0066] The polishing liquid of this comparative example comprises the following components in weight percentage:

[0067] 1 wt% of hydrogen peroxide, 15 wt% of silicon dioxide abrasive (with a particle size of 200 nm), 0.1 wt% of sodium carbonate, 0.1 wt% of sodium carboxymethyl cellulose and the balance being deionized water.

[0068] The polishing method of this comparative example is the same as that of Example 1.

[0069] Comparative Example 2

[0070] The only difference between this comparative example and Example 1 is that no visible light source is used for irradiation.

[0071] Test Case

[0072] 1. The polishing removal rate and roughness test of the silicon carbide obtained after polishing of Examples 1-5 and Comparative Examples 1-2 were performed. The test process is as follows: The surface morphology information of the polished sample is roughly observed by a metallographic microscope, and the surface roughness Ra of the polished sample is analyzed by a ZygoNewView9000 white light interferometer. The polishing removal rate Rr is characterized by a weighing method, which can be calculated by the mass difference of the sample before and after polishing. Let the mass of the sample before polishing be m1, the mass of the sample after polishing be m2, the area of ​​the polished sample be S, and the density be p, then:

[0073]

[0074] Table 1 Polishing removal rate and roughness test results of Examples 1-5 and Comparative Examples 1-2

[0075] Roughness(nm) Removal rate (nm / h) Example 1 0.327 116 Example 2 0.332 138 Example 3 0.314 192 Example 4 0.329 236 Example 5 0.326 362 Comparative Example 1 0.452 73 Comparative Example 2 0.683 92

[0076] According to the test results of Examples 1-5 and Comparative Example 1, as the content of the MIL-125 (Ti) component in Examples 1-5 increases, the removal effect on the silicon carbide sample is greatly improved, up to 362 nm / h, and the roughness can still be maintained at a relatively good level. Compared with Comparative Example 1, Example 5 is improved by nearly 5 times.

[0077] According to the test results of Examples 1-5 and Comparative Examples 1-2, it can be seen from Comparative Example 1 that the removal rate of the polishing liquid without adding MIL-125 (Ti) under visible light irradiation is only 73nm / h, and it can be seen from Comparative Example 2 that after the visible light is turned off, the removal rate of the polishing liquid containing MIL-125 (Ti) decreases from 116nm / h in Example 1 to 92nm / h.

[0078] 2. The polarization curves of the polishing liquids of Example 1 and Comparative Example 1-2 on SiC samples were tested using an electrochemical workstation. The voltage range was 0V to 0.6V and the scanning speed was 1mV / s. The results are shown in the attached figure. Figure 2 As shown, it is found that the polarization curve of Example 1 has the highest corrosion voltage and the smallest corrosion current compared with Comparative Examples 1-2, which proves that the polishing liquid in Example 1 can efficiently generate *OH under light to corrode the silicon carbide sample.

[0079] In summary, compared with Comparative Example 1 in which MIL-125 (Ti) is not added and Comparative Example 2 in which visible light source is not used for irradiation, the present invention adds a titanium-based metal organic framework MIL-125 (Ti) and, under the irradiation of a visible light source, efficiently catalyzes H2O2 to produce a large amount of *OH with a high redox potential, and the generated *OH will not be quenched, which can greatly improve the concentration of *OH and the utilization rate of *OH, so that when polishing SiC, it has a higher *OH to react with the workpiece for oxidation, accelerates the removal of SiC surface materials by abrasives during the polishing process, can effectively improve the polishing efficiency of SiC, has the advantages of high polishing efficiency and few surface defects, and effectively meets the SiC surface polishing quality requirements.

[0080] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A visible light Fenton-chemical mechanical polishing solution for SiC, characterized in that: The composition includes the following weight percentages: 0.02wt% to 0.1wt% of MIL-125 (Ti), 1wt% to 5wt% of hydrogen peroxide, 15wt% to 30wt% of abrasive, 0.1wt% to 0.5wt% of sodium carbonate, 0.1wt% to 0.5wt% of a dispersant and the balance is deionized water.

2. The visible light Fenton-chemical mechanical polishing solution for SiC according to claim 1, characterized in that: The particle size of the MIL-125 (Ti) is 200 nm to 500 nm.

3. The visible light Fenton-chemical mechanical polishing solution for SiC according to claim 1, characterized in that: The abrasive comprises one or both of silicon dioxide and cerium oxide; The particle size of the abrasive is 100nm-500nm.

4. The visible light Fenton-chemical mechanical polishing solution for SiC according to claim 3, characterized in that: The weight ratio of the silicon dioxide to the cerium oxide is (2-10):

1.

5. The visible light Fenton-chemical mechanical polishing solution for SiC according to claim 1, characterized in that: The dispersant includes one or more of sodium carboxymethyl cellulose, sodium hydroxymethyl cellulose and polyvinyl pyrrolidone.

6. A method for preparing a visible light Fenton-chemical mechanical polishing solution for SiC as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: Dissolving a dispersant in deionized water, adding an abrasive and mixing the water to obtain a first suspension; Under yellow light, adding MIL-125(Ti) and sodium carbonate into the first suspension and mixing them to obtain a second suspension; Under yellow light, hydrogen peroxide is added to the second suspension and then mixed in the dark to obtain a visible light Fenton-chemical mechanical polishing solution.

7. A polishing method using the visible light Fenton-chemical mechanical polishing solution as described in any one of claims 1 to 5, or the visible light Fenton-chemical mechanical polishing solution prepared by the preparation method as described in claim 6, characterized in that: The following steps are involved: S1. Injecting the visible light Fenton-chemical mechanical polishing solution between the polishing pad and the SiC at room temperature, and keeping the visible light Fenton-chemical mechanical polishing solution in a dark environment throughout the process; S2. Under the irradiation of a visible light source, the SiC is subjected to visible light Fenton-chemical mechanical polishing, and after the polishing is completed, the SiC is cleaned and dried to obtain a treated SiC.

8. The polishing method according to claim 7, characterized in that: During the visible light Fenton-chemical mechanical polishing process, the rotation speed of the polishing pad is controlled to be 200rpm~1000rpm, and the polishing time is 120min~600min; the material of the polishing pad is damping cloth; the power of the visible light source is 50W~200W; the polishing pressure is 1MPa~10MPa; and the flow rate of the polishing liquid is 1mL / min~5mL / min.